ASTM A240 UNS S32202 Stainless Steel Sheet
What is ASTM A240 UNS S32202 Stainless Steel Sheet?
Equivalent grades: UNS S32202 ≈ EN 1.4062 X2CrNiN22-2 ≈ GB/T 022Cr23Ni2N (S22353).
UNS S32202 is a lean duplex grade. S32202 is a 22Cr-2Ni-N lean duplex grade with almost no molybdenum. Its PREN of about 26 is close to 304L–316L, but its yield strength is more than twice that of austenitic grades. Low nickel keeps the cost stable, so it is mainly used for strength-driven structural and tank applications.
ASTM A240/A240M covers chromium, chromium-nickel and chromium-manganese-nickel stainless steel plate, sheet and strip for pressure vessels and general applications. Under ASTM A480, sheet is flat material under 5.00 mm thick and 600 mm or more wide, so UNS S32202 sheet is a cold-rolled 2B/2D product in thin gauges and a hot-rolled, annealed and pickled No.1 product toward the 4.75 mm end.
This page sets out the ASTM A240/A240M requirements for UNS S32202 sheet: specification summary, chemistry, mechanical properties, corrosion resistance, heat treatment, finishes and tolerances, current stock, equivalents, fabrication and testing. SHH STEEL supplies it mill-direct from China with EN 10204 3.1 certificates, optional third-party inspection and in-house cutting.
UNS S32202 sheet: specification summary
| Item | UNS S32202 data |
|---|---|
| Standard | ASTM A240/A240M; general requirements ASTM A480/A480M |
| ASME counterpart | SA-240 (ordered for ASME Code construction) |
| Product form (A480) | sheet: under 5.00 mm thick, 600 mm and wider; plate 5.00 mm and over |
| Typical gauges | 0.5–3.0 mm cold-rolled 2B/2D; 3.0–4.75 mm hot-rolled No.1 |
| Widths | 1000, 1219, 1250, 1500 mm; slit coil to order |
| Lengths | 2000, 2438, 2500, 3000 mm or cut to size |
| Finishes | No.1, 2D, 2B; BA and No.4 by agreement |
| Required tests | heat analysis, tension test, hardness (and bend where the grade requires it) |
| Certificates | EN 10204 3.1; 3.2 with third-party witness on request |
| Grade family | duplex |
Size range. Sheet is normally cold rolled from about 0.3–0.5 mm up to 3 mm and hot rolled from about 3 mm to just under 5 mm. Coil widths of 1000, 1219, 1250 and 1500 mm are standard; slitting and cut-to-length lines produce narrower strip and exact lengths. Sheets thinner than 0.5 mm or wider than 1500 mm should be confirmed before ordering. UNS S32202 is a specialty grade made by a limited number of mills in campaign rolling. Stock covers the common sizes listed below; for project quantities or unusual sizes, plan for a mill campaign and reserve the heat early.
Chemical composition of UNS S32202 (ASTM A240/A240M)
| Element | wt % |
|---|---|
| C | 0.030 max |
| Si | 1.00 max |
| Mn | 2.00 max |
| P | 0.040 max |
| S | 0.010 max |
| Cr | 21.5–24.0 |
| Ni | 1.00–2.80 |
| Mo | 0.45 max |
| N | 0.18–0.26 |
Single values are maximums unless marked min. Ranges are heat (cast) analysis limits.
PREN check (Cr + 3.3 Mo + 16 N): about 24.4 at the specification minimums and about 27.0 at mid-range. Where corrosion resistance is critical, write a minimum PREN on the order and ask for the calculated value from the heat analysis on the certificate.
Mechanical properties of UNS S32202 sheet
| Condition / thickness | Tensile strength, min | Yield strength 0.2 %, min | Elongation in 50 mm, min | Hardness, max |
|---|---|---|---|---|
| all thicknesses | 650 MPa (94 ksi) | 450 MPa (65 ksi) | 30 % | 290 HBW |
The minimum yield strength of 450 MPa is about 2.6 times the 170 MPa minimum of ASTM 316L. Designers use this to reduce thickness, but higher strength also means higher press loads and more springback. Mill values for production heats are usually well above the minimums; use certificate values when you calculate bending forces. Tension tests are taken in the direction stated in the standard; where a hardness limit is given, it is a maximum that confirms correct annealing.
Corrosion resistance of UNS S32202: PREN and limits
Duplex steels combine about half ferrite and half austenite after solution annealing. The structure gives about twice the yield strength of 304L/316L and much better resistance to chloride stress-corrosion cracking. The PREN (Cr + 3.3 Mo + 16 N) at the specification minimum is about 24.4; a mid-range heat is about 27.0, which places the grade relative to 304L (about 18), 316L (about 24) and 2205 (about 34).
The phase balance depends on correct solution annealing and fast cooling. Too low an annealing temperature or slow cooling can precipitate sigma, chi or chromium nitrides, which cut toughness and corrosion resistance without any visible sign. That is why project specifications add ASTM A923 Method A/B/C tests and a ferrite range. Duplex grades are not recommended for long service above about 300 °C, where 475 °C embrittlement of the ferrite begins.
How UNS S32202 compares with related grades
| Grade | Cr | Ni | Mo | N | PREN (min) | YS / Rp0.2 min, MPa |
|---|---|---|---|---|---|---|
| UNS S32202 | 21.5–24.0 | 1.00–2.80 | 0.45 max | 0.18–0.26 | 24.4 | 450 |
| UNS S82441 | 23.0–25.0 | 3.0–4.5 | 1.00–2.00 | 0.20–0.30 | 29.5 | 540 |
| UNS S32003 | 19.5–22.5 | 3.0–4.0 | 1.50–2.00 | 0.14–0.20 | 26.7 | 485 |
| UNS S32900 | 23.0–28.0 | 2.0–5.0 | 1.00–2.00 | — | 26.3 | 485 |
Choose UNS S32202 when you need more strength and chloride stress-corrosion resistance than 316L at lower cost than super-austenitic or super-duplex grades. Do not use it for long-term service above about 300 °C or where full non-magnetic behaviour is required.
The table uses specification limits, not typical mill values, so it shows the guaranteed position of each grade. Final selection should also consider product availability in the thickness you need, welding consumables, and the inspection requirements of your project.
Heat treatment and delivery condition of UNS S32202
Heat treatment: 980–1080 °C, rapid cooling.
Rapid cooling from the solution-anneal temperature is essential to avoid sigma, chi and chromium nitrides in the 700–1000 °C range. Stress relieving in that range is not allowed; any hot forming must be followed by a full solution anneal and quench.
Surface finishes for UNS S32202 sheet
No.1 is hot-rolled, annealed and pickled, used for the 3–4.75 mm end of the sheet range. 2D is a dull cold-rolled, annealed and pickled finish that holds lubricant in deep drawing. 2B adds a light skin pass for a smoother, brighter surface and is the normal base for polishing. BA (bright annealed) and No.4 brushed finishes are available for many austenitic and ferritic grades by agreement. For highly alloyed grades, cold-rolled thin gauges are produced by fewer mills, so confirm the finish and gauge range before you fix a design.
Dimensions, tolerances and flatness
Thickness, width, length, flatness and camber tolerances follow ASTM A480/A480M. Cold-rolled sheet has tighter thickness tolerances than hot-rolled No.1 sheet. Higher-strength grades show more residual stress after slitting and laser cutting, so for laser blanks or long panels specify flatness and, where needed, tension-levelled material. Edge condition (mill or slit edge) and PVC film on one side should be stated on the order.
Ordering notes for A240 sheet. A240 refers to ASTM A480 for everything that is not grade-specific: definitions of sheet, strip and plate, dimensional tolerances, finishes, marking, retests and certification. A purchase order that says only “A240 S32202” therefore leaves several choices to the mill. State the finish (2B, 2D or No.1), the thickness tolerance basis, whether coil, slit coil or cut lengths are wanted, and whether the certificate must also show SA-240. If the sheet will be formed into vessel heads or pressure parts, say so, because some grades need specific heat-treatment records and supplementary tests that are only reported when requested. For export, also state the edition year if your specification fixes one; most mills certify to the current edition by default.
UNS S32202 sheet stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Finish | Approx. quantity | Location |
|---|---|---|---|---|---|
| 0.5 | 1000 / 1219 | 2000 / 2438 | 2B | 100+ t | China |
| 0.8 | 1219 | 2438 | 2B | 100+ t | China |
| 1.0 | 1219 / 1250 | 2438 / 2500 | 2B | 100+ t | China |
| 1.5 | 1219 / 1500 | 2438 / 3000 | 2B | 100+ t | China |
| 2.0 | 1219 / 1500 | 2438 / 3000 | 2B | 100+ t | China |
| 3.0 | 1500 | 3000 | 2B / No.1 | 100+ t | China |
| 4.0 | 1500 | 3000 / 6000 | No.1 | 100+ t | China |
Quantities are approximate and stock changes daily. Send your size list for current availability; other thicknesses, widths and cut sizes can be supplied from mill production.
Packing and logistics. Sheet is packed on wooden or steel pallets with interleaving paper or PVC film, edge protectors and waterproof wrapping, typically 2–3 t per pallet. Coil is packed eye-to-wall or eye-to-sky with steel bands. We consolidate mixed grades and sizes into one container and send loading photos with the shipping documents.
UNS S32202 equivalents in other standards
| Standard | Designation | Comment |
|---|---|---|
| EN | 1.4062 X2CrNiN22-2 | same alloy family and limits closely matched; compare each limit on the certificate |
| GB/T | 022Cr23Ni2N (S22353) | same alloy family and limits closely matched; compare each limit on the certificate |
Equivalents are close, not identical. When a project names one standard, order to that standard or ask for multiple certification and check every limit on the certificate.
Related grades by alloy family
Duplex and lean duplex
Duplex grades with about twice the yield strength of 316L: A240 S32205, A240 S32304, A240 S32101, 1.4462 plate, 1.4362 plate, A240 S31803, A240 S82441, A240 S32003.
Super duplex
PREN 40+ duplex grades for seawater and severe chlorides: A240 S32750, 1.4410 plate, 1.4501 plate, 1.4507 plate.
Austenitic
General-purpose austenitic grades for comparison: A240 S30400.
Same grade, other specification
Applications, forming and welding of UNS S32202
Typical uses: rebar-replacement structural parts, bridges, storage tanks, water and waste-water equipment, and architectural cladding.
Duplex sheet and plate need about 1.5–2 times the press force of 316L and show more springback. Cut by plasma, laser or waterjet and remove heat tint by pickling or grinding. For welding use a nickel-enriched duplex filler such as ER2209 (AWS A5.9), never an autogenous weld without filler. Keep the weld area clean and free of carbon-steel contamination, and pickle and passivate after welding where corrosion resistance matters.
Welding practice. Keep heat input in the range of about 0.5–2.5 kJ/mm and interpass temperature below about 150 °C. Too low a heat input gives a highly ferritic weld and HAZ; too high a heat input or slow cooling forms intermetallics. Use argon with 1–2 % nitrogen for GTAW where the specification allows, and back-purge root runs. Qualify the procedure with ferrite measurement and, where specified, A923 tests on the weld.
Certificates, testing and receiving inspection
Every delivery carries a mill certificate to ASTM A480/A480M with heat analysis, tensile results and hardness, and the grade and standard as ordered. Supplementary tests we can arrange: ASTM A923 Methods A, B and C, ferrite count to ASTM E562, ASTM G48 pitting test, Charpy impact at the project temperature, and PMI on each plate. Third-party witness by SGS, BV, TÜV, DNV, ABS or LR is available with EN 10204 3.2 certificates.
On receipt, check marking and heat number against the certificate, measure thickness at several points and confirm the finish and edge condition before cutting.
Common mistakes when specifying UNS S32202
- Ordering by UNS number only, without minimum N or PREN, and receiving a heat at the bottom of the range.
- Assuming impact or ferrite requirements from one project apply to all; they come from the project specification, not the product standard.
- Using 2205 design data for a lean duplex grade, or the reverse; strength and PREN differ.
Each of these can be avoided by writing the requirement into the purchase order and checking it on the certificate before the material is cut.
Sourcing UNS S32202: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Phase balance and intermetallics | solution-anneal records checked; A923 and ferrite tests agreed before production |
| Low nitrogen at the bottom of the range | minimum N and PREN written into the order and confirmed from the heat analysis |
| Small quantities across many sizes | mixed thicknesses and grades combined in one shipment |
| Cutting and edge preparation | in-house shearing, plasma, laser and waterjet cutting, bevelling |
| Delivery delays | weekly production and shipping updates with photos |
How to order UNS S32202 sheet
State the standard and edition (ASTM A240/A240M), the grade (UNS S32202), thickness, width and length or coil, finish, quantity, tolerance class, any added chemistry limits, the supplementary tests and acceptance values from your specification, the certificate type and inspection agency, and packing. Send the list to SHH STEEL and we will reply with price, available stock and lead time.
FAQ
-
Can I use A240 S32202 sheet for ASME Code equipment?
- Only if it is certified to SA-240 as well. Most mills dual-certify A240/SA-240; tell us when the sheet is for Code construction and we will supply dual-marked material with the certificate stating both.
-
Is UNS S32202 equivalent to EN 1.4062 X2CrNiN22-2?
- They are the same alloy designation in different standards. Limits are closely matched, but always order to the standard named in your specification or ask for multiple certification.
-
What ferrite range should I specify for UNS S32202?
- Use your project specification. Many specifications ask for 35–55 % ferrite measured to ASTM E562; the product standard itself does not set a range.
-
Can I order small quantities or cut sizes?
- Yes. We combine mixed thicknesses and grades into one shipment and cut plate and sheet to size in our workshop.
-
Which certificates and tests can you provide?
- Every order ships with a mill certificate (EN 10204 3.1 type) showing heat analysis and mechanical tests. Supplementary tests and 3.2 certificates with SGS, BV, TÜV or another agency are available by agreement.
Conclusion
UNS S32202 sheet should be ordered with the points the standard leaves open written into the contract: finish, tolerance class, any extra chemistry limits and the supplementary tests your application needs. With those fixed, stock material from China is a fast and reliable route.