ASME SA553 Type I 9% Nickel Steel Plate
What is ASME SA553 Type I steel plate?
ASME SA553 Type I is water-quenched and tempered 9% nickel alloy steel plate to ASME SA-553/SA-553M. The official split is Type I (9% nickel), Type II (8% nickel) and Type III (7% nickel). This page is Type I only.
ASME BPVC.II.A-2023 prints SA-553/SA-553M as identical with ASTM Specification A553/A553M-17. The current ASTM publication is A553/A553M-22. That identity statement is not a dual-stamp or automatic dual-compliance claim. Orders for Code use should name the Section II edition year, the SA designation and the Type.
SHH STEEL produces and exports ASME SA-553/SA-553M Type I 9% nickel steel plate to the ordered edition, heat treatment, dimensions and extra tests written on the enquiry. This plate belongs to our Boiler & Pressure Vessel Steel Plates range under ASME SA553.
Material specification for ASME SA553 Type I
The items below follow SA-553/SA-553M as printed in ASME BPVC.II.A-2023.
| Parameter | Detail |
|---|---|
| Standard | ASME SA-553/SA-553M, Specification for Pressure Vessel Plates, Alloy Steel, Quenched and Tempered 7, 8, and 9% Nickel |
| Code location | ASME BPVC Section II, Part A. The 2023 edition marks this specification identical with ASTM A553/A553M-17 |
| Official split | Type I (nominal 9% nickel) |
| General requirements | SA-20/SA-20M; SA-553 prevails in a conflict |
| Steelmaking | Killed steel; fine austenitic grain size to SA-20/SA-20M |
| Chemical analysis | Table 1 heat and product analysis for Type I |
| Delivery condition | Water quenched and tempered; marked QT, or QTT when the optional intermediate treatment is used |
| Thickness | Limited only by mechanical properties; see the mill-practice note below |
| Impact testing | Mandatory at −320 °F [−195 °C] unless otherwise agreed; lateral expansion not less than 0.015 in. [0.381 mm] |
| Units | Inch-pound and SI values are separate standards |
| Our supply | We produce and export SA-553 Type I plate to the ordered Code edition, dimensions and extra tests |
Clause 1.4 of the A553/A553M-17 text reproduced as SA-553 in 2023 says that maximum thickness is limited only by the capacity of the material to meet the specified mechanical properties, and it adds that current mill practice normally limits this material to 2 in. [50 mm] maximum. That mill-practice sentence is not a specification thickness ceiling. The public ASTM A553/A553M-22 scope statement does not include the mill-practice sentence.
Types in SA-553/SA-553M:
| Type | Nominal nickel, % | Default impact test temperature |
|---|---|---|
| I | 9 | −320 °F [−195 °C] |
| II | 8 | −275 °F [−170 °C] |
| III | 7 | −320 °F [−195 °C] |
Chemical composition of ASME SA553 Type I
ASME BPVC.II.A-2023 SA-553/SA-553M is marked identical with ASTM A553/A553M-17. The chemical composition, tensile values and heat-treatment temperatures on this page are taken from that 2023 SA-553 text.
The current ASTM publication is A553/A553M-22. It is a separate ASTM document and is supplied when the purchase order names that ASTM edition. This page does not treat an ASTM A553/A553M-22 mark as automatic SA-553 documentation, and it does not treat the 2017 tables as the 2022 ASTM text.
Name the Section II, Part A edition year required by the project, together with SA-553/SA-553M and the Type.
| Element | Type I heat analysis (wt. %) | Type I product analysis (wt. %) |
|---|---|---|
| Carbon (C), max | 0.13 | 0.13 |
| Manganese (Mn), max | 0.90 | 0.98 |
| Phosphorus (P), max | 0.015 | 0.015 |
| Sulfur (S), max | 0.015 | 0.015 |
| Silicon (Si) | 0.15–0.40 | 0.13–0.45 |
| Nickel (Ni) | 8.50–9.50 | 8.40–9.60 |
Carbon, phosphorus and sulfur limits apply to both heat and product analyses. Silicon may be less than the stated heat-analysis minimum of 0.15% if total aluminum is 0.030% or over, or if acid-soluble aluminum is 0.025% or over; the matching product-analysis note allows silicon below 0.13% on the same aluminum basis. Type III is a separate official type in the same table and is specified on its own product page.
Tensile and impact requirements for ASME SA553 Type I
ASME BPVC.II.A-2023 SA-553/SA-553M is marked identical with ASTM A553/A553M-17. The chemical composition, tensile values and heat-treatment temperatures on this page are taken from that 2023 SA-553 text.
The current ASTM publication is A553/A553M-22. It is a separate ASTM document and is supplied when the purchase order names that ASTM edition. This page does not treat an ASTM A553/A553M-22 mark as automatic SA-553 documentation, and it does not treat the 2017 tables as the 2022 ASTM text.
Name the Section II, Part A edition year required by the project, together with SA-553/SA-553M and the Type.
| Property | SA-553/SA-553M (identical with A553/A553M-17) requirement |
|---|---|
| Tensile strength | 100–120 ksi [690–825 MPa] |
| Yield strength (0.2% offset), min | 85 ksi [585 MPa] |
| Elongation in 2 in. [50 mm], min | 20.0% (see SA-20/SA-20M for elongation adjustment) |
| Impact test method | Charpy V-notch to SA-20/SA-20M |
| Specimen orientation | Longitudinal axis of the specimen transverse to the final rolling direction |
| Default test temperature for this type | −320 °F [−195 °C], unless otherwise agreed |
| Mandatory acceptance | Each specimen: lateral expansion opposite the notch not less than 0.015 in. [0.381 mm] |
Optional S55 and S56 energy-absorption requirements apply only when ordered.
Heat treatment for ASME SA553 Type I
Plates are supplied in the water-quenched and tempered condition. Shell plates and other parts heated for forming shall be heat treated after forming to the same procedure.
- Hardening: heat to a suitable temperature in the range 1475–1700 °F [800–925 °C], hold long enough to obtain a uniform temperature through the thickness, and quench in water (the detailed hardening clause also says quench in a liquid medium).
- Tempering 1050–1175 °F [565–635 °C] for Type I: hold at least 30 min/in. [1.2 min/mm] of thickness and not less than 15 min, then cool in air or quench at a rate not less than 300 °F/h [165 °C/h].
Before tempering, plates may receive an optional intermediate heat treatment (1165–1290 °F [630–700 °C] for Type I), held at least 15 min, then cooled as specified by thickness in the standard. When that optional treatment is used, plates are marked QTT instead of QT. The intermediate treatment may be performed at the manufacturer option or specified by the purchaser. This page does not offer heat-treatment or fabrication services.
These temperatures are those of SA-553/SA-553M as printed in ASME BPVC.II.A-2023 (identical with A553/A553M-17). Name the Section II edition year required by the project.
Water quenched and tempered: heat 1475–1700 °F [800–925 °C] and water quench; temper 1050–1175 °F [565–635 °C] for Type I and Type II, hold at least 30 min/in. [1.2 min/mm] and not less than 15 min, then air cool or quench at not less than 300 °F/h [165 °C/h]. Optional intermediate treatment is marked QTT. Temperatures are those of SA-553/SA-553M in ASME BPVC.II.A-2023 (identical with A553/A553M-17).
Welding and handling notes
SA-553 covers plates intended for the fabrication of welded pressure vessels. Welding procedures belong to the Code of construction, the project specification and the fabricator. This page does not offer fabrication or procedure qualification.
The specification warns that the material is susceptible to magnetization after heat treatment.
General requirements, marking and dimensions
Material supplied to SA-553/SA-553M shall conform to SA-20/SA-20M except where SA-553 prevails. Each plate is marked QT, or QTT when the optional intermediate heat treatment is used, in addition to SA-20/SA-20M marking. Dimensional tolerances are those of the ordered SA-20 edition and the mill documents, not a stock list.
Applications and specification limits
We produce and export this plate for projects that specify ASME SA-553/SA-553M Type I. Name the Code of construction and the Section II edition on the order. This page does not claim automatic dual ASTM marking.
Compare ASME SA553 Type I with related nickel steel plates
SA-553 uses the same official Type split as ASTM A553. This page is Type I only. An SA-553 order that omits the Type is incomplete.
| Material | Alloy / type | Delivery condition | Mechanical requirements | Typical service | Substitution limit |
|---|---|---|---|---|---|
| ASME SA553 Type I (this plate) | SA-553 Type I, nominal 9% nickel | Water quenched and tempered; QTT if the optional intermediate treatment is used | Tensile 100–120 ksi [690–825 MPa]; yield 85 ksi [585 MPa] min; impact −320 °F [−195 °C] | Code work that names SA-553 Type I and the applicable Section II edition | Not filled by an ASTM-only A553-22 mark unless the order requires dual documents and both texts are met |
| ASTM A553 Type I 9% nickel steel plate | ASTM A553/A553M-22 Type I | Water quenched and tempered | Same Type I identity in the current ASTM scope; table values on the ASTM page are cited from the -17 / SA-553 text for verification against -22 | Orders written to the current ASTM publication | Related, not an automatic SA stamp. Edition years differ (17 adopted by 2023 Code vs current ASTM 22) |
| ASTM A353 9% nickel steel plate | Double-normalized 9% nickel plate | Double-normalized and tempered | Yield 75 ksi [515 MPa] min; same default −320 °F [−195 °C] impact temperature | ASTM A353 orders | Different heat treatment and yield. Related nickel level only |
| EN 10028-4 X8Ni9 | European 9% nickel grade, 1.5662 | Usually QT on our X8Ni9 page | From our live X8Ni9 page: steel number 1.5662; nickel about 8.50–9.50% (the 8 in X8Ni9 is not 8% nickel); delivery usually quenched and tempered; yield in the 490 MPa class after QT; tensile 640–840 MPa; Charpy specified at −196 °C when the order follows that grade. | EN 10028-4 9Ni plate | Near only; not an SA-553 designation |
| GB/T 713.4-2023 06Ni9DR | Chinese 9% nickel vessel plate | QT or double-QT on our 06Ni9DR page | From our live 06Ni9DR page: current rules in GB/T 713.4-2023 (this name left GB/T 24510-2017 and GB/T 3531-2014); nickel 8.50–10.00%; yield 560 MPa at 5–30 mm; tensile 680–820 MPa; delivery quenched and tempered or double-quenched and tempered; impact −196 °C; lateral expansion not less than 0.64 mm. | GB/T 713.4-2023 9Ni plate | Near only |
| ASME SA203 Grade E | Nickel-alloy pressure-vessel plate in the normalized SA203 family. | Normalized. | Use its own ordered specification, thickness and delivery condition; no strength or toughness value is transferred to this grade. | Low-temperature process vessels and refrigerated containment. | Lower-nickel comparison, not a cryogenic-temperature substitute for ASME SA553 Type I 9% Nickel Steel Plate. Its Code edition, strength, impact temperature and certification must be selected separately. |
Related published ranges: EN 10028-4 and GB/T 713.4-2023.
Equivalent and related grades by country
Near equivalents only. An SA-553 Type order is not filled by a related EN or GB grade name.
| Country / region | Standard | Grade or designation | Similarity and key differences | Substitution caveat |
|---|---|---|---|---|
| United States | ASME SA-553/SA-553M (BPVC.II.A-2023) | Type I | This Code specification, identical with ASTM A553/A553M-17. | This product |
| United States | ASTM A553/A553M-22 | Type I | Current ASTM publication. Not the year adopted by the 2023 Code text. | Related ASTM page; not an automatic SA stamp. |
| United States | ASME SA-353 / ASTM A353 | 9% nickel DNT plate | Same nominal nickel, different heat treatment and yield. | Related family only. |
| Europe | EN 10028-4 | X8Ni9 / X7Ni9 / X10Ni9 | 9% nickel European grades. | Near only. X8Ni9 is 9% nickel. |
| China | GB/T 713.4-2023 | 06Ni9DR | From our live 06Ni9DR page: current rules in GB/T 713.4-2023 (this name left GB/T 24510-2017 and GB/T 3531-2014); nickel 8.50–10.00%; yield 560 MPa at 5–30 mm; tensile 680–820 MPa; delivery quenched and tempered or double-quenched and tempered; impact −196 °C; lateral expansion not less than 0.64 mm. | Near only. |
| Japan | JIS G3127 | 9% nickel plate (SL9N590 cited on our 06Ni9DR page) | Complete official JIS list not restated here. | Near only. |
Why choose SHH STEEL for ASME SA553 Type I
- We produce and export ASME SA-553/SA-553M Type I 9% nickel steel plate
- We review the enquiry for the named standard edition, type or designation, heat treatment, dimensions and any extra tests
- We keep ASTM and ASME orders distinct unless the purchase order requires dual documentation and both texts can be met
- We keep A353 double-normalizing distinct from A553 quenching and tempering, and Type I distinct from Type II
- We match the inspection document to what the purchase order requires
How to enquire for ASME SA553 Type I plate
| Item | What to specify |
|---|---|
| Standard and type | ASME SA-553/SA-553M Type I, plus the Section II, Part A edition year |
| Heat treatment | Water quenched and tempered; say if QTT is required |
| Dimensions | Required thickness, width and length |
| Chemistry | Heat and product analysis for Type I |
| Mechanical tests | Tension to Table 2; Charpy V-notch at −320 °F [−195 °C] unless otherwise agreed |
| Other tests | S55/S56 or NDE only when written on the order |
| Documentation | State the inspection document and any Code marking language required |
| ASTM documents | Request ASTM A553 Type I dual documentation only when the project actually needs it |
Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.
Request a quotation
Contact SHH STEEL for a quotation for ASME SA-553/SA-553M Type I 9% nickel steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.
Specify ASME SA-553/SA-553M Type I and the Section II, Part A edition year. If ASTM A553 Type I dual documents, QTT marking, a non-default impact temperature or NDE are required, include those acceptance criteria.
If you are considering a related European, Chinese or Japanese nickel steel grade as an alternative, send the applicable standard and project specification with your enquiry. We will review the differences in chemistry, heat treatment, impact rules and documentation rather than assume that related grades are interchangeable.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.