ASME SA353 9% Nickel Steel Plate | ASME SA353 Nickel Steel - SHH STEEL

ASME SA353 9% Nickel Steel Plate

ASME SA353 is double-normalized and tempered 9% nickel alloy steel plate under ASME SA-353/SA-353M in Section II, Part A. The 2023 Code edition marks SA-353/SA-353M identical with ASTM A353/A353M-17. That identity statement is not a dual-stamp or automatic dual-compliance claim; Code orders should name the Section II edition and the SA designation. Impact testing is required at −320 °F [−195 °C] unless another temperature is agreed. SHH STEEL produces and exports ASME SA353 9% nickel steel plate to the ordered Code edition and project requirements.
Equivalent Grades:
ASTM A353 / ASME SA353; A553 Type I; EN X8Ni9; GB 06Ni9DR. Conditions, editions and tests differ; not automatic substitutes.
Heat Treatment
Double-normalized and tempered.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
Conclusion

What is ASME SA353 9% nickel steel plate?

ASME SA353 is double-normalized and tempered 9% nickel alloy steel plate to ASME SA-353/SA-353M. There is no Grade, Type or Class split: the specification itself is the 9% nickel double-normalized and tempered plate.

ASME BPVC.II.A-2023 prints SA-353/SA-353M with the statement that it is identical with ASTM Specification A353/A353M-17. That statement describes how that Code edition adopted the ASTM text. It is not a claim that every plate marked ASTM A353 automatically carries SA-353 documentation, and it is not a dual-compliance guarantee from this page. Orders for Code use should name the Section II edition year and the SA designation.

SHH STEEL produces and exports ASME SA-353/SA-353M 9% nickel steel plate to the ordered edition, heat treatment, dimensions and extra tests written on the enquiry. This plate belongs to our Boiler & Pressure Vessel Steel Plates range under ASME SA353.

Material specification for ASME SA353

The items below follow SA-353/SA-353M as printed in ASME BPVC.II.A-2023 and its reference to SA-20/SA-20M.

Parameter Detail
Standard ASME SA-353/SA-353M, Specification for Pressure Vessel Plates, Alloy Steel, Double-Normalized and Tempered 9% Nickel
Code location ASME BPVC Section II, Part A. The 2023 edition marks this specification identical with ASTM A353/A353M-17
Designation system No grade, type or class
General requirements SA-20/SA-20M; SA-353/SA-353M prevails in a conflict
Steelmaking Killed steel; fine austenitic grain size to SA-20/SA-20M
Chemical analysis Heat and product analysis to Table 1
Delivery condition Double-normalized and tempered
Thickness Limited only by the capacity of the material to meet the specified mechanical property requirements
Impact testing Mandatory at −320 °F [−195 °C] unless otherwise agreed; lateral expansion not less than 0.015 in. [0.381 mm]
Units Inch-pound and SI values are separate standards; do not combine them
Our supply We produce and export SA-353 plate to the ordered Code edition, dimensions and extra tests

Chemical composition of ASME SA353 plate

ASME BPVC.II.A-2023 SA-353/SA-353M is marked identical with ASTM A353/A353M-17 and reproduces Table 1 below. Carbon, phosphorus and sulfur limits apply to both heat and product analyses. These figures are the 2023 Code specification table, not an SHH STEEL proprietary chemistry.

Name the Section II, Part A edition year required by the project. The current ASTM publication is A353/A353M-17(2022). An ASTM-only mark is not automatic SA-353 documentation.

Element Heat analysis (wt. %) Product analysis (wt. %)
Carbon (C), max 0.13 0.13
Manganese (Mn), max 0.90 0.98
Phosphorus (P), max 0.015 0.015
Sulfur (S), max 0.015 0.015
Silicon (Si) 0.15–0.40 0.13–0.45
Nickel (Ni) 8.50–9.50 8.40–9.60

The specified silicon minimum does not apply if total aluminum is 0.030% or more, or if acid-soluble aluminum is 0.025% or more. Table 1 may be modified only in accordance with Supplementary Requirement S17 in SA-20/SA-20M when that requirement is invoked.

Tensile and impact requirements for ASME SA353

SA-353/SA-353M Table 2 and clause 7.2, as printed in ASME BPVC.II.A-2023, set the tensile and impact requirements below. One tension test shall be taken from each plate as heat treated.

Property Requirement
Tensile strength 100–120 ksi [690–825 MPa]
Yield strength (0.2% offset), min 75 ksi [515 MPa]
Elongation in 2 in. [50 mm], min 20.0% (see SA-20/SA-20M for elongation adjustment)
Impact test method Charpy V-notch to SA-20/SA-20M
Specimen orientation Longitudinal axis of the specimen transverse to the final rolling direction
Default test temperature −320 °F [−195 °C], unless otherwise agreed
Mandatory acceptance Each specimen: lateral expansion opposite the notch not less than 0.015 in. [0.381 mm]

Optional Supplementary Requirements S55 and S56 add energy-absorption minima and apply only when ordered. They are not the default mandatory impact criterion.

Heat treatment for ASME SA353 plate

All plates shall be heat treated to the double-normalize-and-temper cycle in SA-353/SA-353M. Shell plates and other parts heated for forming shall be heat treated after forming to the same cycle.

  • First normalizing: 1650 ± 25 °F [900 ± 15 °C], hold at least 1 h/in. [2.4 min/mm] of thickness and not less than 15 min, air cool.
  • Second normalizing: 1450 ± 25 °F [790 ± 15 °C], same hold time, air cool.
  • Tempering: 1050–1125 °F [565–605 °C], same hold time, then air cool or water quench at not less than 300 °F/h [165 °C/h].

If hot forming is performed after heating in the range 1650–1750 °F [900–955 °C], the first normalizing treatment may be omitted. This page does not offer heat-treatment or fabrication services.

Double-normalized and tempered: 1650 ± 25 °F [900 ± 15 °C] air cool; then 1450 ± 25 °F [790 ± 15 °C] air cool; temper 1050–1125 °F [565–605 °C], then air cool or water quench at not less than 300 °F/h [165 °C/h]. Hold each stage at least 1 h/in. [2.4 min/mm], and not less than 15 min.

Welding and handling notes

SA-353 covers plates intended particularly for welded pressure vessels for cryogenic service. Welding procedures and any post-weld heat treatment belong to the Code of construction, the project specification and the fabricator. This page does not offer fabrication or procedure qualification.

The specification warns that the material is susceptible to magnetization and that magnets should be avoided in handling after heat treatment if residual magnetism would be detrimental.

General requirements, marking and dimensions

Material supplied to SA-353/SA-353M shall conform to SA-20/SA-20M except where SA-353 prevails. Dimensional tolerances are those of the ordered SA-20/SA-20M edition and the mill documents, not a stock list on this page. Plates shall be descaled by the producer after heat treatment.

Applications and specification limits

We produce and export this plate for projects that specify ASME SA-353/SA-353M. The specification names welded pressure vessels for cryogenic service as the intended use. The applicable Code of construction and Section II edition must be written on the order. This page does not claim an automatic ASTM dual mark.

Compare ASME SA353 with related nickel steel plates

ASME SA-353 is the Section II, Part A material specification for double-normalized and tempered 9% nickel plate. It is published on this site separately from ASTM A353 because an SA designation and an ASTM designation are ordered and documented differently. They are not treated here as identical stamps.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
ASME SA353 9% nickel (this plate) 9% nickel pressure-vessel plate under SA-353/SA-353M; no Type or Class Double-normalized and tempered to SA-353 clause 5.2 Tensile 100–120 ksi [690–825 MPa]; yield (0.2% offset) 75 ksi [515 MPa] min; elongation in 2 in. [50 mm] 20.0% min (SA-20/SA-20M elongation adjustment may apply). Mandatory impact: Charpy V-notch, specimen axis transverse to final rolling, −320 °F [−195 °C] unless agreed otherwise; each specimen lateral expansion opposite the notch not less than 0.015 in. [0.381 mm]. Code work that names SA-353/SA-353M and the applicable Section II edition Do not treat an ASTM-only A353 mark as automatic SA-353 documentation
ASTM A353 9% nickel steel plate ASTM A353/A353M-17(2022) 9% nickel plate Double-normalized and tempered to the same temperature cycle Same Table 1 and Table 2 values as compared between A353/A353M-17(2022) and SA-353 (identical with A353/A353M-17) Orders written to the ASTM specification Related text, different issuing body and edition identifier. Dual compliance only when the order requires it and both documents are met
ASME SA-553 Type I (related QT 9% nickel; separate page) Nominal 9% nickel, Type I Water quenched and tempered Tensile range matches; minimum yield is 85 ksi [585 MPa] rather than 75 ksi [515 MPa] Code work that names SA-553 Type I Different heat-treatment path and yield requirement. Not an SA-353 substitute
EN 10028-4 X8Ni9 European 9% nickel grade, steel number 1.5662 Usually quenched and tempered on our X8Ni9 page From our live X8Ni9 page: steel number 1.5662; nickel about 8.50–9.50% (the 8 in X8Ni9 is not 8% nickel); delivery usually quenched and tempered; yield in the 490 MPa class after QT; tensile 640–840 MPa; Charpy specified at −196 °C when the order follows that grade. EN 10028-4 9Ni vessel plate Near equivalent only; not an ASME SA-353 designation
EN 10028-4 X7Ni9 European 9% nickel sister grade, steel number 1.5663 Usually quenched and tempered on our X7Ni9 page From our live X7Ni9 page: steel number 1.5663; nickel about 8.50–9.50%; tighter carbon band than X8Ni9; usually QT; yield in the 490 MPa class after QT; tensile 640–840 MPa. EN 10028-4 9Ni vessel plate Near equivalent only
GB/T 713.4-2023 06Ni9DR Chinese 9% nickel low-temperature vessel plate Quenched and tempered or double-quenched and tempered on our 06Ni9DR page From our live 06Ni9DR page: current rules in GB/T 713.4-2023 (this name left GB/T 24510-2017 and GB/T 3531-2014); nickel 8.50–10.00%; yield 560 MPa at 5–30 mm; tensile 680–820 MPa; delivery quenched and tempered or double-quenched and tempered; impact −196 °C; lateral expansion not less than 0.64 mm. GB/T 713.4-2023 9Ni vessel plate Near equivalent only. Impact temperature and lateral-expansion floor differ

Related published ranges: EN 10028-4 and GB/T 713.4-2023.

Equivalent and related grades by country

Near equivalents only. An SA-353 order is not filled by naming a related European or Chinese grade, and it is not filled by an ASTM-only mark unless the purchase order requires dual documentation and both texts are met.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United States ASME SA-353/SA-353M (BPVC.II.A-2023) SA-353 / SA-353M This Code material specification, marked identical with ASTM A353/A353M-17. This product
United States ASTM A353/A353M-17(2022) 9% nickel plate Current ASTM publication of the 2017 text, reapproved 2022. Tables compared in this research match the SA-353 reprint. Related ASTM page; not an automatic Code stamp.
United States ASME SA-553/SA-553M Type I Quenched and tempered 9% nickel; higher specified minimum yield. Related, not interchangeable.
Europe EN 10028-4 X8Ni9 / X7Ni9 / X10Ni9 9% nickel European flat-product grades; usually QT on our live pages. Near only. X8Ni9 is not 8% nickel.
China GB/T 713.4-2023 06Ni9DR From our live 06Ni9DR page: current rules in GB/T 713.4-2023 (this name left GB/T 24510-2017 and GB/T 3531-2014); nickel 8.50–10.00%; yield 560 MPa at 5–30 mm; tensile 680–820 MPa; delivery quenched and tempered or double-quenched and tempered; impact −196 °C; lateral expansion not less than 0.64 mm. Near only.
Japan JIS G3127 9% nickel plate (SL9N590 cited on our 06Ni9DR page) Japanese nickel steel plate specification for low-temperature pressure vessels. Complete official grade list not restated here. Near only. No live JIS G3127 product page on this site yet.

Why choose SHH STEEL for ASME SA353 plate

  • We produce and export ASME SA-353/SA-353M 9% nickel steel plate
  • We review the enquiry for the named standard edition, type or designation, heat treatment, dimensions and any extra tests
  • We keep ASTM and ASME orders distinct unless the purchase order requires dual documentation and both texts can be met
  • We keep A353 double-normalizing distinct from A553 quenching and tempering, and Type I distinct from Type II
  • We match the inspection document to what the purchase order requires

How to enquire for ASME SA353 plate

Item What to specify
Standard and designation ASME SA-353/SA-353M, and the Section II, Part A edition year required by the project
Heat treatment Double-normalized and tempered to SA-353
Dimensions Required thickness, width and length
Chemistry Heat and product analysis to Table 1
Mechanical tests Tension to Table 2; Charpy V-notch at −320 °F [−195 °C] unless otherwise agreed
Other tests NDE or S55/S56 only when written on the order
Documentation State the inspection document and any Code marking or certification language required
ASTM documents Request ASTM A353 dual documentation only when the project actually needs it

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

Request a quotation

Contact SHH STEEL for a quotation for ASME SA-353/SA-353M 9% nickel steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the Section II, Part A edition year required by the project and double-normalized and tempered delivery to SA-353/SA-353M. If ASTM A353 documents, a non-default impact temperature, S55/S56 or ultrasonic examination are required, include those acceptance criteria.

If you are considering a related European, Chinese or Japanese nickel steel grade as an alternative, send the applicable standard and project specification with your enquiry. We will review the differences in chemistry, heat treatment, impact rules and documentation rather than assume that related grades are interchangeable.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X