GB/T 4237 12Cr21Ni5Ti (S22160) stainless steel plate at SHH STEEL warehouse

GB/T 4237 12Cr21Ni5Ti S22160 Stainless Steel Plate Supplier

GB/T 4237 12Cr21Ni5Ti (S22160) is an austenitic-ferritic (duplex) stainless steel plate equivalent to 1Cr21Ni5Ti, delivered solution treated. SHH STEEL supplies it hot rolled in 3 – 40 mm, No.1 finish or polished, cut to size, with heat and product analysis on EN 10204 3.1 certificates.
Keywords
12Cr21Ni5Ti, S22160, 1Cr21Ni5Ti, GB/T 4237 12Cr21Ni5Ti, 12Cr21Ni5Ti stainless steel plate, 12Cr21Ni5Ti plate, S22160 stainless steel, 12Cr21Ni5Ti S22160, 12Cr21Ni5Ti supplier
Equivalent Grades:
no direct ASTM / EN / JIS equivalent (Chinese grade, 1Cr21Ni5Ti (Chinese grade)) — Material Specification: GB/T 4237-2015 (12Cr21Ni5Ti, unified code S22160) — Delivery: 950 – 1 050 °C, water or air rapid cooling
Share:
Overview
Specification
Chemical Composition
Product Analysis
Mechanical Properties
Heat Treatment
Corrosion Resistance
Equivalent Grades
Welding & Fabrication
Applications
Grade Comparison
Dimensions
Surface & Processing
Testing & Certificates
Ordering
Mill Sourcing
FAQ
Conclusion

12Cr21Ni5Ti S22160 plate at a glance

12Cr21Ni5Ti (old 1Cr21Ni5Ti) is a Chinese titanium-stabilized duplex developed to save nickel compared with 1Cr18Ni9Ti. Annex B lists it for chemical equipment in the explosives and propellant industries, and for heat exchangers and pipes.

How to read the name: under GB/T 20878 the leading ’12’ is the carbon code (here C 0.09–0.14%), then Cr21 = about 21% chromium; Ni5 = about 5% nickel; Ti = titanium added. S22160 is the unified numeric code (ISC) used in GB/T 4237-2015.

SHH STEEL produces and exports austenitic-ferritic (duplex) stainless plate from China, works as a sales agent for leading stainless mills, and runs its own processing warehouse for cutting and surface finishing. 12Cr21Ni5Ti is part of our GB/T 4237 stainless plate range; for comparison, see our ASTM A240 Type 2205 page.

GB/T 4237 12Cr21Ni5Ti specification details

Item GB/T 4237-2015 requirement / SHH STEEL supply
Standard GB/T 4237-2015 Hot rolled stainless steel plate, sheet and strip (current edition, replaces GB/T 4237-2007)
Grade / unified code 12Cr21Ni5Ti / S22160
Steel class Austenitic-ferritic (duplex)
Chemical composition Table 16 (heat analysis); product analysis per GB/T 222
Mechanical properties Table 21
Product forms Hot-rolled thick plate (3.0 – 200 mm in the standard), hot-rolled wide strip and cut plate (2.0 – 25.4 mm)
Our usual thickness range 3 – 40 mm
Delivery condition 950 – 1 050 °C, water or air rapid cooling
Surface Hot rolled, heat treated, pickled (No.1 / 1D) as standard; ground or polished by agreement
Density 7.7 g/cm³
Certificate EN 10204 3.1 mill certificate; 3.2 with third-party inspection on request

Sister grades on the same standard are listed under GB/T 4237; cold-rolled sheet of the same chemistry is ordered to GB/T 3280, and all our plate lines sit in stainless steel sheets and plates.

Chemical composition of 12Cr21Ni5Ti S22160

Element 12Cr21Ni5Ti heat analysis, % (Table 16) Why it matters
C 0.09 – 0.14 Carbon. Low values protect welds from carbide precipitation; higher values add hot strength or hardenability.
Si ≤ 0.80 Silicon. Deoxidizer; in heat-resistant grades it builds a protective scale.
Mn ≤ 0.80 Manganese. Deoxidizer; in Mn-bearing grades it replaces nickel and keeps nitrogen in solution.
P ≤ 0.035 Phosphorus. Impurity, kept low for toughness and weld cracking resistance.
S ≤ 0.030 Sulfur. Impurity; low sulfur improves pitting resistance, hot workability and polishability.
Cr 20.00 – 22.00 Chromium. Forms the passive film; the main driver of corrosion and oxidation resistance.
Ni 4.80 – 5.80 Nickel. Stabilizes austenite, improves toughness and resistance to reducing acids.
Other Ti: 5 × (C-0.02) – 0.80 Stabilizing / special-element requirement of the standard
PREN (Cr + 3.3Mo + 16N) 20.0 – 21.0 (minimum – mid-range) Calculated from the limits above, not a requirement of GB/T 4237

Values are maximum unless a range is given. The mill reports the ladle (heat) analysis on the certificate; this is the figure to compare with Table 16.

Product (check) analysis tolerances

A check analysis drilled from the finished plate may differ slightly from the heat analysis. GB/T 4237 refers to GB/T 222 for the permitted deviations; the table applies them to the 12Cr21Ni5Ti limits. Deviations apply to one side of a range only, never to both sides in the same heat.

Element Heat analysis limit (%) Permitted deviation Product analysis limit (%)
C 0.09 – 0.14 ±0.01 0.08 – 0.15
Si ≤ 0.80 ±0.05 ≤ 0.85
Mn ≤ 0.80 ±0.03 ≤ 0.83
P ≤ 0.035 +0.005 ≤ 0.040
S ≤ 0.030 +0.005 ≤ 0.035
Cr 20.00 – 22.00 ±0.20 (min) / ±0.25 (max) 19.80 – 22.25
Ni 4.80 – 5.80 ±0.07 (min) / ±0.10 (max) 4.73 – 5.90

Where the table says ‘by agreement’, the deviation is not tabulated for that content level and should be agreed in the contract, usually by reference to ASTM A480 Table A1.1.

12Cr21Ni5Ti S22160 tensile and hardness requirements

Property 12Cr21Ni5Ti (Table 21)
Proof strength Rp0.2, MPa Not specified
Tensile strength Rm, MPa ≥ 635
Elongation A, % ≥ 20

Values apply to plate in the delivery heat-treated condition, tested transversely per GB/T 228.1. Hardness is checked by one method chosen by the mill.

How 12Cr21Ni5Ti plate is heat treated

Recommended heat treatment for 12Cr21Ni5Ti (GB/T 4237-2015 Annex C): 950 – 1 050 °C, water or air rapid cooling.

Follow the annealing window closely; these grades were designed for a specific phase balance.

How 12Cr21Ni5Ti performs in corrosive service

These Chinese duplex grades were developed for oxidizing acids, particularly nitric acid, and for chloride stress corrosion cracking resistance in older chemical plants.

PREN of 12Cr21Ni5Ti from the GB/T 4237 limits: 20.0 – 21.0. PREN is a ranking tool for pitting in chlorides, not a guarantee; temperature, crevices, deposits and weld finish matter as much.

Intergranular corrosion testing is not compulsory for this grade in GB/T 4237-2015; when required, the method (GB/T 4334, ASTM A262 or A923 for duplex) and acceptance are agreed in the order.

If service is harsher than 12Cr21Ni5Ti can handle, the next step up in this batch is GB/T 4237 022Cr23Ni5Mo3N S22053.

International equivalents of 12Cr21Ni5Ti S22160

Standard system Equivalent / closest grade
China GB/T 4237-2015 12Cr21Ni5Ti (S22160)
ASTM A240/A240M —
EN 10088-2 —
JIS G4304 (hot rolled) —
Common name 1Cr21Ni5Ti (Chinese grade)

Equivalent grades are close in chemistry and properties but are never identical: limits on carbon, nitrogen and residual elements differ. For dual or multiple certification the heat must meet every standard named on the order, and we confirm that from the heat chemistry before quotation.

Related pages: ASTM A240 Type 2205. See also our ASTM A240/A240M and JIS G4305 plate lists.

Cutting, forming and welding 12Cr21Ni5Ti plate

Weld with low heat input and matching or 2209-type filler as qualified for the service. These older Chinese grades contain titanium, which can form TiN inclusions in the weld bead; clean joint preparation is essential.

Most users of these grades hold their own qualified procedures from the equipment designer. We supply mill certificates that show the heat chemistry needed for that qualification.

Cutting: we cut 12Cr21Ni5Ti by plasma (up to about 150 mm), laser (thin plate) or waterjet, and remove the heat-affected edge by machining where the drawing requires it.

Typical uses of GB/T 4237 12Cr21Ni5Ti

Applications listed in GB/T 4237 Annex B and in practice:

  • Nitric acid and chemical equipment
  • Explosive and propellant plant parts
  • Heat exchangers and pipes as a 321 substitute

Buyers specifying 12Cr21Ni5Ti for these jobs often compare it with GB/T 4237 14Cr18Ni11Si4AlTi S21860 and GB/T 4237 022Cr23Ni5Mo3N S22053; the comparison table on this page shows the differences.

International grade pages for the alternatives mentioned above: ASTM A240 Type 321.

Other GB/T 4237 grades buyers request alongside it: GB/T 4237 022Cr22Ni5Mo3N S22293, GB/T 4237 022Cr25Ni7Mo4N S25073, GB/T 4237 022Cr23Ni4MoCuN S23043, GB/T 4237 022Cr23Ni2N S22353, GB/T 4237 022Cr25Ni6Mo2N S22553, GB/T 4237 022Cr25Ni7Mo4WCuN S27603.

Choosing between 12Cr21Ni5Ti and its neighbours

The table compares 12Cr21Ni5Ti with the grades buyers most often weigh it against. Strength values are GB/T 4237-2015 minimums; PREN is calculated from the minimum chemistry.

Grade (GB/T 4237) Key chemistry, % PREN min Rp0.2 min, MPa Rm min, MPa
12Cr21Ni5Ti S22160 C 0.09 – 0.14, Cr 20.00 – 22.00, Ni 4.80 – 5.80 20.0 — 635
GB/T 4237 14Cr18Ni11Si4AlTi S21860 C 0.10 – 0.18, Cr 17.50 – 19.50, Ni 10.00 – 12.00, Si 3.40 – 4.00, Ti 0.40 – 0.70 17.5 — 715
GB/T 4237 06Cr18Ni11Ti S32168 C ≤ 0.08, Cr 17.00 – 19.00, Ni 9.00 – 12.00, N ≤ 0.10 17.0 205 515
GB/T 4237 022Cr23Ni5Mo3N S22053 C ≤ 0.030, Cr 22.00 – 23.00, Ni 4.50 – 6.50, Mo 3.00 – 3.50, N 0.14 – 0.20 34.1 450 655

High carbon (0.09–0.14%) and titanium make this an older-design grade; most new projects specify 2205 or 2304. Mill-order item.

12Cr21Ni5Ti plate sizes

Dimension Typical supply
Thickness 3 – 40 mm
Width 1 000 / 1 219 / 1 250 / 1 500 / 1 800 / 2 000 mm; wider by mill order
Length 2 000 / 2 438 / 3 000 / 6 000 mm or cut to size
Flatness Per GB/T 4237; ≤15 mm per metre for plate up to 25 mm unless agreed tighter
Thickness tolerance Per the GB/T 4237 dimensional tolerance tables (normal or higher accuracy as ordered)
Edge Mill edge or cut edge

Weight: plate mass in kg/m² = thickness (mm) × density (7.7 g/cm³). A 10 mm 12Cr21Ni5Ti plate weighs about 77.0 kg/m²; a 1 500 × 6 000 × 10 mm plate about 693 kg.

Finishes and warehouse services

Finish Description Availability for this grade
No.1 / 1D Hot rolled, heat treated, pickled; the GB/T 4237 standard surface Standard
Shot-blasted + pickled Uniform matte for welded structures On request
Ground Ground surface for defect removal or UT On request
2B / BA Cold-rolled finishes (ordered as GB/T 3280 sheet, not hot-rolled plate) Sheet only

Our warehouse cuts plate to size (plasma, laser, waterjet, saw), bevels weld edges, polishes and applies PVC protective film. Processed plate ships with the original mill heat number marked. Ask for cut pieces of other stainless steel products at the same time to consolidate freight.

Quality documents supplied

  • Heat chemical analysis on every heat; product analysis by agreement
  • Tensile test (Rp0.2, Rm, A) per batch
  • Hardness test
  • Ferrite content measurement
  • ASTM A923 Method A/B/C for intermetallic phases when specified
  • Charpy V-notch impact at −40 °C or −46 °C when specified
  • Ultrasonic testing (NB/T 47013.3 or ASTM A578) when specified
  • Positive material identification (PMI) on every plate leaving our warehouse
  • Visual and dimensional inspection; third-party inspection (SGS, BV, TÜV, Intertek) at the buyer’s request

Certificates follow EN 10204 3.1 as standard. Where plate is also certified to ASME SA240 or ASTM A240, both standards are shown on one certificate.

What to put on a 12Cr21Ni5Ti purchase order

  • Standard and edition: GB/T 4237-2015
  • Grade and code: 12Cr21Ni5Ti (S22160); add the equivalent if dual certification is needed
  • Thickness × width × length, quantity in pieces or tonnes
  • Thickness tolerance class and flatness if tighter than standard
  • Surface finish and protective film
  • Tests beyond the standard (IGC, UT, impact, ferrite, PMI, grain size)
  • Certificate type (EN 10204 3.1 / 3.2) and inspection body
  • Marking, packing (wooden cases, steel pallets) and delivery terms

Send the list to SHH STEEL and we return a quotation with mill, lead time and stock options. Other grades from the same standard can be combined in one shipment; browse GB/T 4237 plate grades.

Mill sourcing and lead time

12Cr21Ni5Ti is produced by a small number of Chinese mills with the melting and heat treatment capability for it. We place mill orders for it through the producers we represent and do not usually hold it in stock. Expect about 45–90 days, with minimum quantities per thickness; we can combine small quantities into one rolling where the mill allows.

Every plate is traceable to its heat number, and copies of the mill certificates stay on file for repeat orders and audits. The same mills also supply our ASTM A240, ASME SA240, JIS G4305 and AISI plate ranges, so mixed-standard orders can ship together.

FAQ

Is 12Cr21Ni5Ti a duplex steel?
Yes. 12Cr21Ni5Ti (S22160, old 1Cr21Ni5Ti) is listed among the austenitic-ferritic grades in GB/T 4237-2015 (Table 16). It is a Ti-stabilized Chinese grade with Cr 20–22% and Ni 4.8–5.8%, with no direct ASTM or EN equivalent.
What is the chemical composition of 12Cr21Ni5Ti?
Under GB/T 4237-2015 Table 16, 12Cr21Ni5Ti (S22160) has C 0.09 – 0.14, Cr 20.00 – 22.00, Ni 4.80 – 5.80; Ti: 5 × (C-0.02) – 0.80. Phosphorus is limited to ≤0.035% and sulfur to ≤0.030%.
What are the mechanical properties of 12Cr21Ni5Ti plate?
GB/T 4237-2015 Table 21 requires for 12Cr21Ni5Ti: tensile strength ≥635 MPa and elongation ≥20%. Values apply to plate in the delivery heat-treated condition.
Is 12Cr21Ni5Ti stainless steel magnetic?
Yes, partly. Duplex plate contains about 50% ferrite, so it attracts a magnet, though less strongly than ferritic steel.
What thickness of 12Cr21Ni5Ti plate can you supply?
Under GB/T 4237 we supply 12Cr21Ni5Ti hot-rolled plate in 3 – 40 mm, widths up to 2 000 mm (wider by mill order), cut to size in our warehouse. Thinner material is cold-rolled sheet to GB/T 3280.
What is the PREN of 12Cr21Ni5Ti?
Using PREN = Cr + 3.3Mo + 16N and the GB/T 4237-2015 limits, 12Cr21Ni5Ti has a PREN of about 20.0 at minimum chemistry and 21.0 at mid-range.

Conclusion

GB/T 4237 12Cr21Ni5Ti (S22160) is a Chinese-developed duplex plate grade, formerly designated 1Cr21Ni5Ti and without a direct foreign equivalent. It is defined by Table 16 chemistry (C 0.09 – 0.14, Cr 20.00 – 22.00, Ni 4.80 – 5.80) and Table 21 properties. Typical uses include nitric acid and chemical equipment, explosive and propellant plant parts and heat exchangers and pipes as a 321 substitute. High carbon (0.09–0.14%) and titanium make this an older-design grade; most new projects specify 2205 or 2304.

Before ordering, state the standard edition, the grade name with its code, and any extra tests, so that the mill certificate matches your design documents. SHH STEEL supplies 12Cr21Ni5Ti plate by mill order through the producers we represent, cut to size and finished in our own warehouse, with EN 10204 3.1 certificates. For related grades see GB/T 4237 14Cr18Ni11Si4AlTi S21860 and GB/T 4237 06Cr18Ni11Ti S32168, our GB/T 4237 category and the ASTM A240 Type 2205 page. Send your sizes and quantities for a quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X