RINA FH32 Shipbuilding Steel Plate
RINA FH32 shipbuilding steel plate — overview
RINA FH32 is the −60 °C grade of the 32 level and uses the tighter F-column chemistry: lower C, P and S, a nitrogen limit and more room for Ni. Level 32 is the entry high-tensile level. It is popular on ferries and superyachts, where a modest strength gain over mild steel trims weight high up in the ship without changing welding practice much. Minimum yield is 315 N/mm², tensile 440–590 N/mm², elongation 22 %.
Equivalent grades: ASTM A131 Grade FH32 · ABS FH32 · DNV NV F32 · LR FH32 · BV FH32 · CCS F32 / FH32 · NK KF32 · KR RF32 · GB 712 Grade FH32.
In RINA’s high-tensile series the letter sets the Charpy temperature (AH 0 °C, DH −20 °C, EH −40 °C, FH −60 °C) and the number sets the yield (32 → 315, 36 → 355, 40 → 390 N/mm²). FH32 is the F letter at level 32. Typical RINA-classed uses: polar expedition cruise ships, Arctic ice-class tonnage and cold-region offshore units whose design temperature calls for −60 °C.
RINA is the Genoa-based society that classes much of the Italian fleet and a large share of the world’s cruise ships and ferries, many of them built at Fincantieri and other Italian and Mediterranean yards. That background shows in the steel: passenger ships use large areas of thin plate in decks and superstructure, so flatness, weld distortion and consistent supply count as much as the grade letter.
SHH STEEL supplies FH32 from Chinese mills whose RINA approval covers high-tensile hull steel in the ordered condition and thickness, with the RINA survey at the mill. Common 36-level sizes are held in stock; the rest is rolled to order.
How RINA names it. For higher-strength steel RINA uses the IACS form: H for high tensile, the toughness letter in front and the strength level behind, so FH32 = letter F, level 32. Buyers sometimes shorten it to “F32”, but on RINA paperwork the H stays.
Level 32 gives about a third more yield than mild steel at a small price premium, and its weldability is close to mild steel, so it is an easy first step for yards moving superstructure or ferry decks to high-tensile.
RINA FH32: key data at a glance
| Item | RINA FH32 |
|---|---|
| Rule book | RINA Rules for the Classification of Ships, Part D (Materials and Welding), higher-strength hull steel; IACS UR W11 FH32 (RINA numbering not quoted — UNCERTAIN) |
| Designation | FH32: toughness letter FH + strength level 32 |
| Strength | ReH ≥ 315 N/mm², Rm 440–590 N/mm², A ≥ 22 % |
| Charpy V | −60 °C |
| Steelmaking | killed and fine-grain treated (Al, Nb, V or Ti) |
| Condition of supply | AR / CR / N / TM as permitted by thickness and grain refiner; QT where approved |
| TM carbon equivalent | Ceq ≤ 0.36 % (t ≤ 50 mm), ≤ 0.38 % (50–100 mm) — indicative UR W11 practice, confirm on approval |
| Thickness scope | up to 100 mm (UR W11); beyond by agreement with RINA |
| Minus tolerance | IACS UR W13 (confirm class — UNCERTAIN) |
| Certificate | RINA-endorsed mill certificate; EN 10204 3.1 / 3.2 |
Traded FH32 is usually 6–60 mm thick and 2000–3000 mm wide. FH plate above about 50 mm is offered by fewer mills, so check the approval range before you fix the design thickness.
RINA FH32 chemistry — full alloy list
| Element | Ladle (heat) analysis, % | Product (check) analysis, % | Comment |
|---|---|---|---|
| C | 0.16 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | FH column |
| Si | 0.10–0.50 | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| Mn | 0.90–1.60 | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| P | 0.025 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | F column tighter |
| S | 0.025 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | F column tighter |
| Al (acid-soluble) | 0.015 min. acid-soluble | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | grain refiner |
| Nb | 0.02–0.05 when used singly | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | grain refiner / strength |
| V | 0.05–0.10 when used singly | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| Ti | 0.02 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| Cu | 0.35 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| Cr | 0.20 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| Ni | 0.80 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | larger allowance in F column |
| Mo | 0.08 max. | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | |
| N | 0.009 max. (0.012 if Al present) | numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate | cap applies to F column |
| Nb+V+Ti | 0.12 max. (combined, when used together) | not applicable (calculated from heat analysis) | combined microalloy cap |
| Ceq (TM plate) | 0.36 / 0.38 max. (calculated) | not applicable (calculated from heat analysis) | t ≤ 50 / 50–100 mm |
Product (check) analysis column: RINA Rules Part D specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.
Ladle limits are the IACS UR W11 values for higher-strength hull steel, applied by RINA in Part D (not checked against a RINA edition — UNCERTAIN). The F column caps C at 0.16 %, P and S at 0.025 % and N at 0.009 % (0.012 % with Al), and allows Ni up to 0.80 %. Check each of these on the certificate.
For TM plate ask for Ceq on the certificate, and Pcm too if your welding procedure is qualified on it. At level 32, most mills reach the strength with Nb alone. Check-analysis tolerances are agreed case by case.
RINA FH32 tensile requirements
| Property | Requirement |
|---|---|
| ReH | 315 N/mm² min. |
| Rm | 440–590 N/mm² |
| A (5.65√S0) | 22 % min. |
| Charpy test temperature | −60 °C |
Flat 200 mm test pieces — minimum elongation by thickness:
| t (mm) | ≤5 | 5–10 | 10–15 | 15–20 | 20–25 | 25–30 | 30–40 | 40–50 |
|---|---|---|---|---|---|---|---|---|
| A200 min. % | 14 | 16 | 17 | 18 | 19 | 20 | 21 | 22 |
AH32, DH32, EH32 and FH32 share these tensile values; only the Charpy temperature and, for FH, the chemistry differ. Compared with mild steel, FH32 gives 80 N/mm² more yield, which is the margin the designer spends on thinner plate.
Tensile specimens are taken transverse to the rolling direction for plate wider than about 600 mm, as UR W11/W16 practice requires; the certificate should show the specimen orientation. For TM plate, a yield/tensile ratio is often around 0.8–0.9; there is no class limit unless the order adds one (indicative).
RINA FH32: Charpy at −60 °C and condition of supply
| Thickness | Avg. long. (J) | Avg. trans. (J) |
|---|---|---|
| ≤ 50 mm | 31 | 22 |
| 50–70 mm | 38 | 26 |
| 70–100 mm | 46 | 31 |
Required energy rises with thickness: a 70–100 mm FH32 plate must average 46 J longitudinal at −60 °C, against 31 J up to 50 mm. FH plate is almost always TM or N; as-rolled plate rarely meets −60 °C reliably.
Condition of supply sets batch size and test frequency, so it belongs on the order. If the owner’s specification adds strain-aged impact tests or Z-direction properties, those are extra requirements and must be priced and booked in advance.
Thickness tolerance and surface
The minus tolerance follows IACS UR W13 as RINA applies it; plus tolerance, flatness and dimensions follow the agreed standard (EN 10029 or GB/T 709). Weight-optimised high-tensile designs — and passenger ships are among the most weight-sensitive — leave little margin, so measure thickness at several points on receipt. Thin high-tensile deck plate distorts more easily during welding than thicker plate; ordering a tighter flatness class can save fairing work later.
UR W13 also allows local grinding of surface defects and sets how the average thickness of a plate is checked; the measurement points and acceptance method should be agreed at enquiry if the yard has its own procedure. For RINA passenger-ship work we suggest stating both the minus tolerance class and the flatness class on the order for any plate under 10 mm.
RINA FH32 stock and lead time
| Thickness (mm) | Width (mm) | Length (mm) | Condition | Approx. qty |
|---|---|---|---|---|
| 5 | 1500 / 1800 | 6000–12000 | AR / N / TM | 80+ t |
| 6 | 1800 / 2000 | 6000–12000 | AR / N / TM | 100+ t |
| 8 | 2000 | 6000–12000 | AR / N / TM | 150+ t |
| 10 | 2000 / 2200 | 6000–12000 | AR / N / TM | 200+ t |
| 12 | 2000 / 2500 | 6000–12000 | AR / N / TM | 200+ t |
| 16 | 2200 / 2500 | 6000–12000 | AR / N / TM | 150+ t |
| 20 | 2500 | 6000–12000 | AR / N / TM | 120+ t |
| 25 | 2500 | 6000–12000 | AR / N / TM | 100+ t |
| 30 | 2200 / 2500 | 6000–12000 | AR / N / TM | 80+ t |
| 40 | 2200 | 6000–12000 | AR / N / TM | 50+ t |
| 50 | 2200 | 6000–12000 | AR / N / TM | 30+ t |
Quantities change weekly — confirm before booking. Plates are sold as RINA FH32 with the RINA mark and endorsed certificate. Anything outside the stock list goes into the next mill campaign: about 4–6 weeks to certified plate.
Packing: bundled by size with steel strapping, marked with grade and heat number, shipped in containers (≤ 11.8 m) or break bulk to Mediterranean and other ports.
Processing before shipping. We cut FH32 to drawing by plasma or oxy-fuel, bevel edges for welding, shot-blast and prime with shop primer, and mark each piece with grade, heat number and part number so that RINA traceability survives cutting. Cut parts ship with a cutting list that cross-references every piece to its original plate and certificate.
RINA FH32 against other class societies
| Society / standard | Designation | Remark |
|---|---|---|
| RINA | RINA FH32 | this page — Rules for the Classification of Ships, Part D |
| BV | BV FH32 | closest naming habit (A/B/D/E, AH…, A420…) |
| DNV | DNV VL F32 | VL prefix |
| LR | LR FH32 | |
| ABS | ABS FH32 | |
| CCS | CCS F32 / FH32 | |
| KR | KR RF32 | R-prefix |
| NK | NK KF32 | K-prefix |
| ASTM A131 | ASTM A131/A131M Grade FH32 | product standard, no class stamp |
| GB 712 | GB 712 Grade FH32 | Chinese product standard, no class stamp |
All of these share the UR W11 FH32 requirements. Each society accepts only its own mark, so if you need RINA plus a second society, book both surveyors before the plates are tested.
Where FH32 sits in the RINA AH/DH/EH/FH matrix
Think of the series as a grid: moving right (AH32, DH32, EH32, FH32) lowers the test temperature, moving down (FH32, FH36, FH40) raises the yield. The RINA material class table fixes the letter from structural category and thickness; the scantling calculation fixes the number. Substituting a higher letter at the same number is normally accepted; a lower letter is not.
FH32 is chosen for polar and Arctic service. Few designs need it outside ice-class tonnage, so check that the class table really asks for −60 °C before paying for it. Above 390 N/mm², RINA’s extra-high-strength series starts at F420 (IACS UR W16). See RINA Steel Plates.
Level 32 is often chosen for thinner upper decks and superstructure fronts where buckling, not yield, governs, so the full 355 N/mm² of level 36 would not be used.
Welding and forming RINA FH32
Typical uses: polar expedition cruise ships, Arctic ice-class tonnage and cold-region offshore units whose design temperature calls for −60 °C.
Welding: use RINA-approved high-tensile consumables of grade 5Y or higher (typical UR W17 mapping — confirm in the WPS). Preheat and heat input follow the RINA-approved procedure and the Ceq on the certificate. High-heat-input electrogas or one-side submerged-arc welding of thick FH32 needs a procedure qualified at that heat input.
Forming: TM plate gets part of its strength from controlled rolling and cooling. Keep line heating within the mill’s temperature limit — typically quoted around 650 °C for accelerated-cooled plate (UNCERTAIN, mill-specific).
Why the F letter here. FH32 is tested at −60 °C and is chosen for polar and Arctic service and the coldest design temperatures. FH plate needs the tightest steelmaking control, so certificates should be checked line by line for P, S, N and Ni. When building blocks mix letters, keep FH32 plates physically separated and colour-marked in the yard so that a lower letter is never fitted by mistake.
RINA survey, certificate and receiving checks
The certificate lists ladle chemistry including microalloys, Ceq for TM plate, tensile results, Charpy results at −60 °C, condition of supply and plate numbers, with the RINA surveyor’s endorsement.
On receipt: check the stamp reads FH32 with the RINA mark, the Charpy temperature and thickness band match the plate, and the endorsement is present. We can add EN 10204 3.2 witness, UT to EN 10160 or ASTM A578, Z-direction tests and dual class with another IACS society.
RINA approval of the manufacturer. A mill is approved by RINA for named grades, steelmaking route, delivery condition and maximum thickness, after approval tests and periodic renewal. Before placing an order for FH32, ask to see that the approval scope actually lists this grade and condition up to the thickness you need — this is the single most useful check a buyer can make (approval document format UNCERTAIN).
Mistakes we see on RINA FH32 orders
- Writing only “FH32” without RINA, so the plate arrives with another society’s mark
- Leaving the letter off (“36 grade”), so toughness is undefined
- Accepting a normal-strength A/B/D/E certificate against a high-tensile order
- No Ceq on the certificate for TM plate
- Substituting AH32 without class approval
- F-column limits (N, P, S, Ni) not checked
A clear order line — grade, rule book, condition, certificate — prevents nearly all of them.
With FH32 the expensive errors are mixed letters within a delivery, missing Ceq for TM plate, and plates whose thickness falls into a higher Charpy band than the test covered.
Buying RINA FH32 from China: concerns and answers
| Concern | Answer |
|---|---|
| Is the RINA mark genuine? | Only mills with RINA approval for RINA FH32; certificate and stamp traceable to the heat; third-party witness on request |
| Can the surveyor at our yard verify it? | Yes — the certificate number and heat can be checked against the mill’s RINA records |
| Payment safety | T/T with balance after inspection, or L/C at sight |
| Small or mixed orders | several sizes and RINA grades in one container |
| Delivery visibility | weekly photos from rolling to loading |
| Ready-to-fit parts | cutting, bevelling and drilling in our own workshop |
If your yard has never bought from a Chinese mill under RINA survey, we can arrange a trial lot, share sample certificates in advance, and let your inspector or the RINA surveyor visit the mill during rolling and testing.
Ordering RINA FH32
State: RINA FH32, condition of supply, sizes and quantities, UT / Z-direction, dual class, certificate type and port, and send to SHH STEEL.
Sample line: “Hull plate to RINA Rules for the Classification of Ships, Part D, grade FH32, TM, 12 × 2500 × 12000 mm, 40 pcs, RINA-endorsed certificate with Ceq, EN 10204 3.2, CFR Monfalcone.”
Order checklist:
- Society and rule book: RINA Rules for the Classification of Ships, Part D
- Grade: FH32
- Condition of supply (AR / N / TM as allowed)
- Sizes and quantity per size; flatness class if tighter than standard
- Certificate: RINA-endorsed, EN 10204 3.1 or 3.2
- Extras: UT, Z-direction, dual class, shot-blast/prime, cutting
- Delivery terms and destination port
FAQ
Conclusion
RINA FH32 is higher-strength hull steel under RINA’s Rules for the Classification of Ships, Part D (Materials and Welding): yield 315 N/mm², tensile 440–590 N/mm², Charpy −60 °C. A RINA-classed ship accepts it only with the RINA mark and an endorsed certificate.
SHH STEEL supplies RINA FH32 from RINA-approved Chinese mills, with cutting, UT and EN 10204 3.2 on request. Send grade, sizes, quantities and port for a quotation.