RINA E500 extra-high-strength hull plate to RINA Rules Part D / IACS UR W16: ReH 500 N/mm², Charpy −40 °C, TM or QT. Mill-rolled at RINA-approved Chinese mills via SHH STEEL, with UT and 3.2 inspection.
Keywords
RINA E500 steel plate, RINA Grade E500, Registro Italiano Navale E500, RINA E500 extra high strength hull steel, UR W16 marine plate
Equivalent Grades:
BV E500; DNV VL E500; LR EH50; ABS EH50 / EQ51; CCS EH500; KR RE51; NK KE500; GB 712 EH500
Share:
Overview
Specification
Chemical Composition
Mechanical Properties
Impact Test and Condition of Supply
Thickness Tolerance
Stock
Equivalent Grades
Grade Selection
Applications and Fabrication
Testing and Inspection
Specification Mistakes
Buyer Concerns
How to Order
FAQ
Conclusion

RINA E500 extra-high-strength shipbuilding steel plate — overview

Technical Reviewer: Jack | SHH STEEL Material Solutions Department · Updated: 2026-10-28

RINA E500 combines 500 N/mm² minimum yield with −40 °C Charpy toughness. RINA names its extra-high-strength hull steels in the official form without an “H”: toughness letter A, D, E or F followed by the minimum yield in N/mm², so E500 rather than an AH-style name. They are covered in Part D (Materials and Welding) of the Rules for the Classification of Ships on the basis of IACS UR W16. The 500 level is mainly an offshore and special-vessel level; mainstream merchant hulls rarely go this high.

Equivalent grades: ASTM A131 (no direct grade at this strength) · ABS EH50 / EQ51 · DNV NV E500 · LR EH50 · BV E500 · CCS EH500 · NK KE500 · KR RE51 · GB 712 Grade EH500.

UR W16 values: ReH ≥ 500 N/mm², Rm 610–770 N/mm², A ≥ 16 %, Charpy at −40 °C. The E letter is the usual choice for primary offshore members and for crack-arrest areas, where −40 °C is the design basis.

E500 is produced TM or QT, and only at a mill whose RINA approval names this grade, condition and thickness range. Approval for AH36 or for a lower EHS level does not extend to it automatically.

Extra-high-strength plate is less common on RINA’s core passenger-ship work than AH/DH36, but it appears on the largest ships, on cranes and lifting gear, and widely on offshore and special units classed by RINA.

E500 is rolled to order, not held as open stock. SHH STEEL places the order with a RINA-approved Chinese mill, books the RINA survey, and adds UT, dual class or 3.2 witness on request. Typical uses: offshore units, heavy-lift and special vessels; seldom mainstream merchant hulls.

How RINA names it. For extra-high-strength steel RINA drops the H and writes the yield in full — E500 — which is why the same plate appears as EH500 in IACS UR W16 and some product standards. Both describe the same 500 N/mm² level with −40 °C toughness.

RINA E500: key data at a glance

Item RINA E500
Rule book RINA Rules for the Classification of Ships, Part D (Materials and Welding), extra-high-strength steel; IACS UR W16 (RINA numbering not quoted — UNCERTAIN)
Designation E500: toughness letter E + minimum yield 500 N/mm² (official form, no “H”)
Strength ReH ≥ 500, Rm 610–770 N/mm², A ≥ 16 %
Charpy V −40 °C; average ≥ 50 J L / 33 J T (UR W16-aligned — confirm)
Condition of supply TM or QT within the approved thickness (N only if specifically approved)
Steelmaking killed, fine-grain; vacuum degassing and Ca treatment typical
UT normally specified for this class — agree standard and acceptance level
Minus tolerance IACS UR W13 (confirm class)
Certificate RINA-endorsed certificate including Ceq / CET / Pcm; EN 10204 3.2 on request

Maximum thickness is set by the mill approval. As a guide, TM E500 is often approved to about 50–80 mm and QT thicker, but the approval certificate is the limit (UNCERTAIN). At this level, most enquiries are 20–100 mm QT plate for offshore and lifting structure.

RINA E500 chemistry — full alloy list including B

Element Ladle (heat) analysis, % Product (check) analysis, % Comment
C 0.21 max. (often 0.14–0.20 by route/condition; TM/QT may tighten) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Si 0.55 max. (QT may allow up to ~0.80 — confirm on mill approval) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Mn 1.70 max. (typically 1.00–1.70; QT route may differ) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
P 0.025 max. (some EQ-style routes tighter — confirm) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
S 0.025 max. (some EQ-style routes tighter — confirm) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Al 0.015 min. acid-soluble / ≈0.020 total Al (fine-grain; Al/N control unless other N-binders) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate grain refiner / N binder
Nb 0.05 max. (when used; combined microalloy caps apply) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
V 0.10 max. (when used; combined caps apply) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Ti 0.05 max. (when used; combined caps apply) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Cu 0.50 max. (route-dependent; often ≤0.35 in practice) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Cr 0.20–0.25 max. (route-dependent) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Ni 2.00 max. or per mill approval (often lower on AH/DH routes) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate toughness
Mo 0.08–0.50 (route-dependent; QT may allow higher) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate hardenability (QT)
B 0.005 max. (when intentionally added) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate hardenability (QT)
N 0.015 max. (tighter control when Al is the sole N-binder) numeric tolerance not tabulated in RINA Rules Part D – agree on order / mill certificate
Nb+V+Ti Nb+V+Ti typically < 0.26 % for N/TM routes (not QT) — confirm UR W16 / mill approval not applicable (calculated from heat analysis) combined
Ceq / CET / Pcm Ceq / CET / Pcm maxima by category and condition on mill approval — report on certificate not applicable (calculated from heat analysis) calculated

Product (check) analysis column: RINA Rules Part D specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.

The table gives the UR W16 envelope. RINA fixes the exact limits for each mill at approval, so the approval document and the order govern (UNCERTAIN against the Part D text). From 500 upward, Ni and Mo become regular additions and the heavier gauges are made QT.

The E letter at this level shares the A/D/E chemistry envelope; the toughness difference comes mainly from process route and steel cleanliness. Every intentionally added element must appear on the certificate together with Ceq, CET or Pcm, because the welding procedure depends on them.

Boron, when added, works in parts per million and is effective only when nitrogen is tied up, usually by titanium; that is why B, Ti and N should be read together on the certificate.

RINA E500 tensile and impact requirements

Property Requirement
ReH (or Rp0.2) 500 N/mm² min.
Rm 610–770 N/mm²
A 16 % min.
Charpy V −40 °C, ≥ 50 J L / 33 J T (average)
Yield/tensile ratio report; limit only if specified on the order

Tests are taken per heat-treatment batch or per rolled length as the approval requires; thick plate may need extra mid-thickness tests. Compared with EH40 the yield rises by 110 N/mm². That gain only pays off if the welded joint keeps up, so check that the qualified procedure reaches matching strength and toughness in weld metal and HAZ, not just in the plate.

Tensile specimens are taken transverse to the rolling direction for plate wider than about 600 mm, as UR W11/W16 practice requires; the certificate should show the specimen orientation. For QT plate, Rp0.2 is often reported instead of ReH because the yield point is not pronounced.

RINA E500: toughness at −40 °C and TM vs QT

Charpy specimens are normally taken at quarter thickness and tested at −40 °C. Delivery is TM or QT; the choice changes mill, price, flatness and welding behaviour, so state it on the order. QT is the usual route at this level, particularly in thick plate; TM may be possible in thinner gauges where the approval allows.

At this toughness level many owners also ask for CTOD or brittle-crack-arrest data. Those are separate requirements (UNCERTAIN), so specify them if you need them.

TM plate gets its strength from controlled rolling and accelerated cooling, so it starts with low carbon and good weldability, but can lose some strength if heated above the mill’s limit. QT plate is austenitised, quenched and tempered, which gives uniform properties in thick sections; the tempering temperature then becomes the ceiling for any later heat treatment.

Thickness tolerance and flatness

Minus tolerance follows IACS UR W13; plus tolerance and flatness follow the agreed standard. QT plate is generally flatter than heavy TM plate but harder to straighten afterwards, so agree the flatness class at enquiry. Do not flame-straighten EHS plate above the mill’s stated temperature without approval — it can undo the TM or tempering treatment.

UR W13 also allows local grinding of surface defects and sets how the average thickness of a plate is checked; the measurement points and acceptance method should be agreed at enquiry if the yard has its own procedure. For EHS plate, thickness is usually measured by ultrasonic gauge at the mill and recorded on request; ask for it if the design relies on the minimum thickness.

RINA E500 mill-rolled supply

Thickness (mm) Width (mm) Condition Typical lot
12 2000 / 2500 TM / QT per heat / rolling
16 2200 / 2500 TM / QT per heat / rolling
20 2500 TM / QT per heat / rolling
25 2500 TM / QT per heat / rolling
30 2200 / 2500 TM / QT per heat / rolling
40 2200 TM / QT per heat / rolling
50 2200 TM / QT per heat / rolling

RINA E500 is not held as open stock. The table shows the thickness and width combinations we most often book into a mill campaign; expect roughly 6–10 weeks from order to RINA-certified plate (commercial estimate).

Packing: bundled by size with steel strapping, marked with grade and heat number, shipped in containers (≤ 11.8 m) or break bulk to Mediterranean and other ports.

Processing before shipping. We cut E500 to drawing by plasma or oxy-fuel, bevel edges for welding, shot-blast and prime with shop primer, and mark each piece with grade, heat number and part number so that RINA traceability survives cutting. Cut parts ship with a cutting list that cross-references every piece to its original plate and certificate.

RINA E500 against other class societies

Society / standard Designation Remark
RINA RINA E500 this page — Rules for the Classification of Ships, Part D
BV BV E500 closest naming habit (A/B/D/E, AH…, A420…)
DNV DNV VL E500 VL prefix
LR LR EH50 EHS numbered by yield/10
ABS ABS EH50 / EQ51 commercial / official
CCS CCS EH500
KR KR RE51 R-prefix
NK NK KE500 K-prefix
ASTM A131 none A131 stops at FH40
GB 712 GB 712 Grade EH500 Chinese product standard, no class stamp

All sit in the same UR W16 band. The names differ (with or without “H”, R- or K-prefix, LR yield/10 numbers), and only the RINA mark counts for a RINA-classed structure.

Where E500 sits in the RINA A420–F690 series

Neighbours are E460 below and E550 above. Within level 500 the letter sets the test temperature: A 0 °C, D −20 °C, E −40 °C, F −60 °C. Changing level needs RINA plan approval.

As a rough guide for a yield-governed member, 30 mm of EH40 becomes about 23.4 mm of E500. Buckling, fatigue and corrosion margins often limit the real saving, so the gain is usually smaller (estimate, not a rule value).

Other RINA grades are listed under RINA Steel Plates; offshore-specific grades under offshore platform steel plates.

In RINA practice, EHS grades are usually concentrated in a few highly stressed areas rather than used everywhere. That keeps the number of welding procedures down: the yard only needs E500 procedures for the members where it pays.

Fabricating RINA E500

Typical uses: offshore units, heavy-lift and special vessels; seldom mainstream merchant hulls.

The yard welds E500 only under a RINA-approved WPS qualified on this grade, using low-hydrogen consumables that reach matching strength and −40 °C toughness in the weld metal. Heat input must be limited to protect HAZ toughness in QT plate, and preheat is usually needed on thick sections. Do not hot-form or stress-relieve above the tempering temperature without agreement from the mill and RINA.

Why the E letter here. E500 is tested at −40 °C and is chosen for crack-arrest areas, ice-class ships and cold-region service. Owners of passenger ships often specify EH for sheer strakes and deck stringers regardless of thickness, as an added safety margin. When building blocks mix letters, keep E500 plates physically separated and colour-marked in the yard so that a lower letter is never fitted by mistake.

HAZ softening can occur in TM plate under very high heat input, and HAZ hardening in QT plate under very low heat input, so the qualified range in the WPS should be respected on both sides. Hydrogen control — dry consumables, clean joints and controlled preheat — matters more as strength rises.

RINA survey, certificate and receiving checks

The certificate gives full alloy analysis, Ceq/CET/Pcm, tensile results, −40 °C Charpy results, condition of supply, UT result and plate numbers, with the RINA surveyor’s endorsement.

On receipt, check the E500 stamp and RINA mark, impact temperature, UT report and endorsement. Dual class with another IACS society and 3.2 witness are available if booked before testing.

RINA approval of the manufacturer. A mill is approved by RINA for named grades, steelmaking route, delivery condition and maximum thickness, after approval tests and periodic renewal. Before placing an order for E500, ask to see that the approval scope actually lists this grade and condition up to the thickness you need — this is the single most useful check a buyer can make (approval document format UNCERTAIN).

Mistakes we see on RINA E500 orders

  • Writing AH500 instead of the official E500, or leaving out RINA
  • Leaving TM vs QT open
  • No UT requirement
  • Ceq/Pcm not requested
  • Ordering from a mill whose RINA approval does not cover the grade or thickness
  • Expecting an ASTM A131 dual certificate (none exists at this level)

EHS plate is rolled for you, so a wrong order line costs a full rolling cycle. Check it twice.

With EHS plate the expensive errors are the ones that cannot be fixed after rolling: wrong route, wrong thickness range for the mill approval, or missing UT.

Buying RINA E500 from China: concerns and answers

Concern Answer
Is the RINA mark genuine? Only mills with RINA approval for RINA E500; certificate and stamp traceable to the heat; third-party witness on request
Can the surveyor at our yard verify it? Yes — the certificate number and heat can be checked against the mill’s RINA records
Payment safety T/T with balance after inspection, or L/C at sight
Small or mixed orders sizes grouped onto one heat where possible
Delivery visibility weekly photos from rolling to loading
Ready-to-fit parts cutting, bevelling and drilling in our own workshop

If your yard has never bought from a Chinese mill under RINA survey, we can arrange a trial lot, share sample certificates in advance, and let your inspector or the RINA surveyor visit the mill during rolling and testing.

Ordering RINA E500

State RINA E500, TM or QT, sizes and quantities, UT level, dual class, certificate type and port, and send to SHH STEEL.

Sample line: “Plate to RINA Rules for the Classification of Ships, Part D, grade E500, QT, 40 × 2500 × 10000 mm, 8 pcs, UT EN 10160 S1E1, RINA-endorsed certificate with Pcm, EN 10204 3.2.”

Order checklist:

  • Society and rule book: RINA Rules for the Classification of Ships, Part D
  • Grade: E500
  • Condition of supply (TM or QT)
  • Sizes and quantity per size; flatness class if tighter than standard
  • Certificate: RINA-endorsed, EN 10204 3.1 or 3.2
  • Extras: UT, Z-direction, dual class, shot-blast/prime, cutting
  • Delivery terms and destination port

FAQ

Why is it E500 and not AH500?
For extra-high-strength steel RINA uses the official form without “H”: toughness letter plus minimum yield, so E500. IACS UR W16 and some other standards write EH500. It is the same strength and toughness level, but use E500 on a RINA order so that the stamp and certificate match the drawing. Its −40 °C test temperature makes it suitable for crack-arrest areas, ice-class ships and cold-region service. At 500, check that the mill approval covers both the grade and the thickness you need. The no-H form also avoids confusion with commercial short names; on RINA drawings and certificates use E500 and add “(UR W16 EH500)” in brackets if your purchasing system needs the IACS form. Write the society on every document: plates without the RINA mark will be rejected at the yard however good the results are.
What does E500 guarantee?
ReH ≥ 500 N/mm², Rm 610–770 N/mm², A ≥ 16 % and a Charpy average of at least 50 J longitudinal or 33 J transverse at −40 °C (UR W16-aligned; confirm on the certificate). Chemistry limits are fixed in the mill’s RINA approval. Owners of passenger ships often specify EH for sheer strakes and deck stringers regardless of thickness, as an added safety margin. For the E letter the test temperature is −40 °C; the energy requirement itself is the same across letters at level 500. At 500 N/mm² yield the tensile window 610–770 N/mm² is wide; ask the mill for typical results on the thickness you order to judge consistency. EH plate is the usual crack-arrest grade, so expect the owner’s specification to ask about it specifically.
TM or QT — which should I order for E500?
QT is the usual route at this level, especially in thick plate; TM is possible in thinner gauges where the approval allows. The route changes price, flatness and the welding procedure, so state it on the order and make sure the yard’s WPS was qualified on the same route. At −40 °C, mills usually control sulphur and inclusion shape closely to secure consistent results. Ask the mill which route its RINA approval covers for your thickness. For E500, TM is uncommon at this strength, and QT also gives more uniform through-thickness properties in heavy plate. The approved drawing and the RINA material class table decide; the purchase order should simply repeat what the drawing says.
Is E500 available from stock?
Rarely. E500 is rolled to order at a mill whose RINA approval covers this exact grade and thickness, typically in 6–10 weeks including survey. Grouping sizes onto one heat keeps cost and test count down. E500 consumables must also meet −40 °C toughness in the weld metal. At 500, check that the mill approval covers both the grade and the thickness you need. Order planning matters: a rolling slot is booked first, then survey, then shipping, so confirm drawings early. We can send a sample certificate for E500 before you order so your quality department can check the format.
Which elements appear on the certificate?
C, Si, Mn, P, S, Al, Nb, V, Ti, Cu, Cr, Ni, Mo, B and N where added, plus Nb+V+Ti and Ceq, CET or Pcm. Weldability depends on all of them, so a certificate that leaves out B or Pcm on QT plate should be queried. Substitution by a higher letter is a quality upgrade; the cost difference should be agreed before delivery. Missing elements on a QT certificate are a common reason for rejection at the yard. Pcm is especially relevant for low-carbon QT chemistries, where Ceq can understate hardening tendency; your WPS should state which index is used. For EHS, ask for mill approval evidence covering the exact thickness.
Where is E500 used?
Typical uses at this level: offshore units, heavy-lift and special vessels; seldom mainstream merchant hulls. The E letter fits members whose design calls for −40 °C toughness; the RINA material class table decides that from category and thickness. Marks of other societies are added only if requested at order stage. EHS members are usually identified on the approved drawing with the full grade name. On RINA-classed offshore units, EHS plate is usually concentrated in legs, chords, racks, crane pedestals and highly stressed nodes; the hull plating is typically still AH/DH36. Your WPS should be qualified on the same grade, thickness range and delivery route.
What welding precautions apply to E500?
A RINA-approved procedure qualified on this grade, low-hydrogen consumables of matching strength and toughness, controlled preheat and heat input, and no post-weld heat or flame straightening above the tempering or mill-stated temperature. Plates for crack-arrest areas, ice-class ships and cold-region service are often specified with Z-direction properties at joints loaded through thickness. Preheat values come from the WPS, not from generic tables. For QT plate, keep preheat and interpass temperatures within the WPS range and avoid excessive heat input, which can soften or embrittle the HAZ. Thickness and width affect price as much as grade, so send the full size list for an accurate quote.
What are payment terms and inspection options?
Usually a T/T deposit with the balance paid once inspection is passed, or an irrevocable L/C at sight. UT, EN 10204 3.2 witness and dual class with another IACS society can be added if booked before testing. Ask for a pro-forma invoice and inspection plan together, so payment milestones match testing. Partial shipments by heat are possible on larger orders. Inspection at the mill can be combined with UT witnessing to save one visit; book both before rolling. Prices are usually quoted per tonne, with extras for cutting, priming, UT and 3.2 inspection itemised separately.

Conclusion

RINA E500 is extra-high-strength hull steel under RINA’s Rules for the Classification of Ships, Part D (Materials and Welding): yield 500 N/mm², tensile 610–770 N/mm², Charpy −40 °C. A RINA-classed ship accepts it only with the RINA mark and an endorsed certificate.

SHH STEEL supplies RINA E500 from RINA-approved Chinese mills, with cutting, UT and EN 10204 3.2 on request. Send grade, sizes, quantities and port for a quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X