KR RD32 Shipbuilding Steel Plate
KR RD32 (KR RD32) shipbuilding steel plate — overview
KR RD32 is the Korean Register higher-strength grade with Charpy at −20 °C (IACS UR W11 equivalent DH32). KR plan approval on Korean-built tankers and container ships assigns RD32 to thicker deck, bottom and sheer strakes where 0 °C is not enough. Strength level 32 means minimum yield 315 N/mm², tensile 440–590 N/mm² and elongation 22 % min. (A5). The letter D fixes Charpy V-notch testing at −20 °C. In commercial enquiries it is called KR RD32 shipbuilding steel plate; “KR DH32” is a common but unofficial way of writing it.
Equivalent grades: KR RD32 ≈ ASTM A131 Grade DH32 ≈ ABS DH32 ≈ DNV NV D32 ≈ LR DH32 ≈ BV DH32 ≈ CCS D32 / DH32 ≈ NK KD32 ≈ RINA DH32 ≈ GB 712 Grade DH32 (all class-approved, stamped by the issuing society).
KR RD32 is selected when the scantling needs the 32 yield band and the KR material class assigns −20 °C toughness. Ordinary-strength KR RA–RE stay at 235 N/mm² and cannot replace RD32 without a drawing change. In the KR ladder for strength 32: RA32 0 °C → RD32 −20 °C → RE32 −40 °C → RF32 −60 °C; within the D letter, RA32 → RA36 → RA40-style steps raise yield from 315 to 355 to 390 N/mm².
Plates that pass mill tests under KR survey are stamped with the KR mark and RD32 (stencils sometimes add the IACS form DH32 for the yard; plus Z or U where through-thickness or ultrasonic requirements apply) and are supplied with a mill certificate the KR Surveyor endorses. SHH STEEL supplies KR RD32 from Chinese mills that hold KR works approval for the grade, from stock in common sizes or from a mill rolling cycle, with KR survey arranged at the mill.
KR RD32 plate: specification summary
| Item | KR RD32 / RD32 data |
|---|---|
| Rule basis | KR Rules Pt 2; IACS UR W11 higher-strength Grade DH32 (KR Rules Pt 2 paragraph cross-refs UNCERTAIN without local KR Rules text) |
| Official KR designation | RD32 (R prefix = KR rolled hull steel); IACS / ABS-style equivalent DH32 — write RD32 on KR-class POs |
| Related product standard | ASTM A131/A131M Grade DH32 — product standard only; not KR class approval |
| Strength level | higher strength 32, yield 315 N/mm² min., tensile 440–590 N/mm² |
| Toughness class | DH / R → Charpy at −20 °C |
| Plate thickness primarily covered | up to 100 mm under IACS UR W11 scope for plates; greater thickness by special consideration (see UNCERTAIN) |
| Deoxidation | killed, fine grain practice (UR W11) |
| Impact test | Charpy V at −20 °C; frequency and supply condition per UR W11 / KR Rules Pt 2 tables |
| Marking | KR RD32 / KR RD32; plus Z / U / TM where ordered and qualified |
| TMCP Ceq (indicative UR W11 / industry practice) | ≤ 0.36 % for t ≤ 50 mm; ≤ 0.38 % for 50 < t ≤ 100 mm (TM steels) — confirm on mill approval / PO |
| Thickness tolerance | IACS UR W13 as adopted by KR (minus tolerance commonly 0.3 mm class — confirm on PO; see UNCERTAIN) |
| Certificate | mill certificate endorsed by the KR Surveyor; EN 10204 3.1 / 3.2 on request |
Size range. Common market thicknesses for RD32 are about 6–80 mm (heavier plates available as per mill approval), widths 1500–3500 mm. Exact maximum thickness for a given delivery condition is as per standard and mill certificate / KR works approval. Ask for confirmation above 100 mm.
KR RD32 (KR RD32) chemical composition (heat and product analysis)
| Element | Heat (ladle) analysis, % | Product (check) analysis, % | Note |
|---|---|---|---|
| C | 0.18 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | AH/DH/EH group |
| Mn | 0.90–1.60 (AH ≤12.5 mm may be 0.70 min.) | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | AH ≤12.5 mm may use 0.70 % Mn min. |
| Si | 0.10–0.50 | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | min. waived if acid-soluble Al ≥ 0.015 % |
| P | 0.035 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | |
| S | 0.035 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | |
| Al (acid soluble) min. | 0.015 min. acid-soluble (or total Al per UR W11 fine-grain practice) | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | grain refining |
| Nb | 0.02–0.05 when used singly | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | when used singly; combined minima in UR W11 |
| V | 0.05–0.10 when used singly | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | when used singly |
| Ti | 0.02 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | need not be reported unless intentionally added |
| Cu | 0.35 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | |
| Cr | 0.20 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | |
| Ni | 0.40 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | |
| Mo | 0.08 max. | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | |
| N | — | numeric tolerance not tabulated in KR Rules (Part 2) – agree on order / mill certificate | not specified as a max in AH/DH/EH column |
Product (check) analysis column: KR Rules (Part 2) specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.
Source: IACS UR W11 higher-strength chemistry tables (ladle samples), adopted by Korean Register for KR RD32 in Rules for the Classification of Steel Ships Pt 2 (KR paragraph numbers UNCERTAIN). The full grain-refining and residual set (Al, Nb, V, Ti, Cu, Cr, Ni, Mo, N) is shown so you can check every row on the certificate. AH/DH/EH share one chemistry column; FH is tighter on C, P, S and adds N control with higher Ni allowance. Toughness is differentiated by impact temperature and supply routes, not by separate C/Mn caps within AH/DH/EH. Product (check) analysis numeric tolerances are not tabulated in UR W11; when required, agree tolerances at enquiry. TMCP steels must also meet the applicable Ceq / Pcm limits on the mill approval — ask for Ceq on the certificate.
KR RD32 tensile properties
| Property | Requirement (IACS UR W11) |
|---|---|
| Tensile strength Rm | 440–590 N/mm² |
| Yield strength ReH | 315 N/mm² min. |
| Elongation A5 | 22 % min. |
| Impact test temperature | −20 °C |
Alternative flat-specimen elongations by thickness (indicative UR W11 / industry table for strength 32):
| Thickness (mm) | ≤5 | >5–10 | >10–15 | >15–20 | >20–25 | >25–30 | >30–40 | >40–50 |
|---|---|---|---|---|---|---|---|---|
| Elongation min. % | 14 | 16 | 17 | 18 | 19 | 20 | 21 | 22 |
Same tensile band applies to A/AH, D/DH, E/EH and F/FH 32; only impact temperature and chemistry group (FH vs AH/DH/EH) change across the letter.
KR RD32: Charpy at −20 °C and supply condition
| Thickness | Long. avg. at −20 °C | Trans. avg. at −20 °C |
|---|---|---|
| t ≤ 50 mm | 31 J | 22 J |
| 50 < t ≤ 70 mm | 38 J | 26 J |
| 70 < t ≤ 100 mm | 46 J | 31 J |
Source: IACS UR W11 impact table for higher-strength Grade DH32 (full-size; either direction acceptable unless specified). Energies rise with thickness — a 60 mm plate must meet higher values than a 20 mm plate at the same −20 °C. Condition of supply and impact lot size depend on grain-refining practice and thickness (AR/CR/N/TM/QT as permitted). For TMCP RD32, respect Ceq caps ≈ 0.36 % (t≤50) / 0.38 % (50
Thickness tolerance and surface condition
Korean Register applies IACS UR W13 thickness tolerances unless the PO states otherwise (often 0.3 mm minus class — confirm on PO; see UNCERTAIN). Plus/flatness/width/length per agreed standard (ASTM A6, EN 10029 or GB/T 709). Surface quality per EN 10163 or equivalent accepted by KR; state primer/surface class on receipt if needed.
KR RD32 plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Condition | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1800 / 2000 | 6000 / 8000 | AR / CR / N / TM | 100+ t | China |
| 8 | 1800 / 2000 | 8000 / 12000 | AR / CR / N / TM | 200+ t | China |
| 10 | 2000 / 2200 | 8000 / 12000 | AR / CR / N / TM | 200+ t | China |
| 12 | 2000 / 2200 / 2500 | 12000 | AR / CR / N / TM | 200+ t | China |
| 14 | 2000 / 2200 | 12000 | AR / CR / N / TM | 100+ t | China |
| 16 | 2000 / 2500 | 12000 | AR / CR / N / TM | 200+ t | China |
| 20 | 2000 / 2500 | 12000 | AR / CR / N / TM | 100+ t | China |
| 25 | 2200 / 2500 | 12000 | AR / CR / N / TM | 100+ t | China |
| 30 | 2200 | 10000 / 12000 | AR / CR / N / TM | 100+ t | China |
| 40 | 2200 | 10000 | AR / CR / N / TM | 50+ t | China |
| 50 | 2200 | 8000 / 10000 | AR / CR / N / TM | 50+ t | China |
Quantities are approximate and change daily (indicative — confirm before booking); all stock plates carry KR RD32 marking and KR-endorsed mill certificates when sold as KR class plate. Sizes outside the table (for example 3000 mm width, 60–100 mm thickness, or fixed lengths for a cutting plan) are produced in the next mill rolling cycle, typically 3–6 weeks including KR survey. Send your size list and we will reply with what is in stock and what must be rolled.
Packing. Plates are bundled by size with steel strapping, marked with heat number, grade and KR stamp, and shipped in containers (up to about 11.8 m) or break bulk for longer plates.
KR RD32 equivalents in other rules and standards
| Standard / society | Designation | Comment |
|---|---|---|
| KR (Korean Register) | KR RD32 | this page; official KR designation RD32 (IACS DH32); stamped under KR survey |
| GB 712 | GB 712 Grade DH32 | Chinese product standard; not class approval by itself |
| ASTM A131/A131M | ASTM A131/A131M Grade DH32 | A131 lists AH–FH 32/36/40; product standard only |
| ABS | ABS DH32 | IACS UR W11 higher-strength; live product page |
| DNV | DNV NV D32 | IACS UR W11; live product page |
| LR | LR DH32 / LR/DH32 | IACS UR W11; live product page |
| BV | BV DH32 | IACS UR W11; live product page |
| NK (ClassNK) | NK KD32 | ClassNK KD32 |
| CCS | CCS D32 / DH32 | IACS UR W11; live CCS product page |
| RINA | RINA Grade DH32 | confirm exact designation per RINA rules |
| Structural (indicative) | S275JR | land structural; no class marking |
These are comparisons, not substitutions. Multi-class stamps (KR + ABS / DNV / LR / BV) require joint survey before rolling. Other KR siblings in the 32 band are linked via KR until each product page is live.
KR RD32 vs other KR hull grades
Pick RD32 when the drawing specifies higher-strength grade DH32 (KR writes DH32 as RD32). Do not substitute ordinary Grade A/B unless the designer recalculates scantlings — yield differs (315 vs 235). Within the 32 band, letter choice is toughness: A/AH 0 °C → D/DH −20 °C → E/EH −40 °C → F/FH −60 °C. Within the DH letter, strength steps 32 → 36 → 40 raise yield from 315 to 355 to 390 N/mm².
For yields above 390 N/mm² KR moves to extra-high strength (IACS UR W16): RA43…RF70, numbered by ABS-style yield class (420 → 43 … 690 → 70; UNCERTAIN vs local KR text) rather than CCS/DNV DH420 or BV A420.
When KR RD32 is the right choice: typical uses are higher-strength members that the material class table assigns to −20 °C, such as thicker deck and bottom strakes, sheer strakes and hatch coamings. The Charpy temperature (−20 °C) is fixed by the letter, and the strength by the number (ReH 315 N/mm²). Pick the strength from the scantling calculation and the letter from the material class and design temperature on the approved drawing.
Applications, cutting and welding of KR RD32
Typical uses: higher-strength members that the material class table assigns to −20 °C, such as thicker deck and bottom strakes, sheer strakes and hatch coamings; weight-saving vs ordinary-strength plate in large tankers, bulkers and container ships built to KR class. See offshore platform steel plates when primary offshore grades apply.
Welding: higher-strength hull steels need approved higher-strength consumables matched to −20 °C weld-metal toughness; preheat and heat input follow the approved WPS and often track Ceq/Pcm from the mill certificate. TMCP RD32 must respect the Ceq caps noted above. Cutting by oxy-fuel/plasma/laser is routine; thick FH plate may need hydrogen control — follow mill recommendations.
Processing notes for KR RD32: cold forming is routine within normal shipyard radii. Line heating and fairing of TMCP plate should stay within the temperature limits recommended by the mill, because overheating can reduce the strength gained in controlled rolling. Check the delivery condition on the certificate before planning hot forming.
Certificates, KR survey and third-party inspection
Every plate is tested and marked at the mill under Korean Register survey; the mill certificate lists heat number, ladle chemistry, Ceq where applicable, tensile results (ReH ≥ 315 N/mm², Rm 440–590 N/mm², A ≥ 22 %), Charpy at −20 °C, delivery condition and plate numbers, endorsed by the Surveyor. Optional EN 10204 3.2, UT (U), Z-direction, multi-class with ABS/DNV/LR/BV.
On receipt: verify KR RD32 (or KR RD32) stamp, −20 °C impact data, energies for the delivered thickness band, thickness within UR W13 / PO tolerance, KR Surveyor endorsement present — not a mill-only certificate.
Charpy acceptance for KR RD32 by thickness (IACS UR W11; actual results as per standard and mill certificate):
| Thickness t (mm) | Test temperature | Average energy, longitudinal (J min.) | Average energy, transverse (J min.) |
|---|---|---|---|
| t ≤ 50 | −20 °C | 31 | 22 |
| 50 < t ≤ 70 | −20 °C | 38 | 26 |
| 70 < t ≤ 100 | −20 °C | 46 | 31 |
If UT or 3.2 was ordered, check the UT report and inspector’s plate list as well.
Common mistakes when ordering KR RD32 (KR RD32)
- Ordering “KR 32” without the letter — toughness class missing
- Writing DH32 (ABS/CCS style) on a KR PO without stating KR RD32 — the KR certificate and stamp read RD32
- Accepting ordinary-strength Grade A/B certificates for a RD32 PO
- Accepting a DH32 certificate from another society (or a product-standard paper) where KR RD32 is specified
- Ignoring TMCP Ceq caps on TM plate
- Substituting a different letter (e.g. AH for DH) without drawing approval
- Coil-cut plate without coil approval
- Missing KR endorsement on the MTC
- Writing DNV NV D32 or LR/DH32 on a KR-class PO without arranging that society’s survey
Write the KR grade (RD32), delivery condition, impact temperature and certificate type into the PO.
Sourcing KR RD32: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Fake class plate | KR-approved mills only; traceable KR RD32 stamp + certificate; 3.2 on request |
| Payment risk | T/T or L/C; inspection before balance |
| Mixed sizes / grades | RD32 combined with KR Grade A/B/D/E or other A–FH sizes in one container |
| Lead time visibility | weekly photo updates from dedicated coordinator |
| Prep before ship | cutting, bevelling, drilling, machining in our workshop |
How to order KR RD32 plate
Specify KR RD32 (KR RD32), delivery condition (AR/CR/N/TM/QT as applicable), thickness × width × length × qty, Z/U, multi-class, certificate type, port. Send to SHH STEEL.
Sample PO line: “Steel plate to KR Rules for the Classification of Steel Ships, Pt 2, Grade RD32 (KR RD32), delivery condition [AR/CR/N/TM/QT], 20 × 2500 × 12000 mm, 30 pcs, marked KR RD32, certificate endorsed by KR Surveyor, EN 10204 3.2 [if required], UT [if required], CIF [port].”
FAQ
Conclusion
KR RD32 / KR RD32 is higher-strength hull steel under KR Rules for the Classification of Steel Ships, Pt 2 and IACS UR W11: yield 315 N/mm², tensile 440–590 N/mm², Charpy at −20 °C, marking KR RD32. DH32 is the cross-society name for the same IACS grade, but only the KR RD32 stamp and KR-endorsed certificate are accepted for KR class. Lock on the order: delivery condition, impact lot size, TMCP Ceq if TM, product analysis if needed, multi-class and 3.2.
SHH STEEL supplies KR RD32 plate rolled by Chinese mills that hold Korean Register works approval for the grade, so every plate carries the KR RD32 stamp and a Surveyor-endorsed certificate traceable to its heat. Common thicknesses are available from stock; other sizes are scheduled into the mill rolling cycle with KR survey arranged at the mill. On request we add EN 10204 3.2 certificates with third-party witness (TÜV, SGS, LR or another agency) and joint certification with ABS, DNV, LR, BV, NK, KR or RINA.
We accept T/T or L/C payment, with inspection before the balance is paid. Small quantities in several sizes, or KR RD32 mixed with KR RA/RB/RD/RE or other RA–RF 32/36/40 sizes, can be combined in one container. A dedicated coordinator sends production and shipping updates with photos, and our own workshop cuts to size, bevels, drills and machines plates before shipment so they arrive ready for fabrication.
Request a quotation: send SHH STEEL the grade (KR RD32 / KR RD32), thickness, width, length, quantity per size and destination port, plus any multi-class, Z/U or 3.2 certificate requirement. We reply with price, available stock and lead time.