JIS G3127 SL9N590 Steel Plate | JIS G3127 Steel - SHH STEEL

JIS G3127 SL9N590 Steel Plate

JIS G 3127 SL9N590 is a quenched-and-tempered 9 % nickel steel plate for cryogenic pressure vessels. Heat-analysis nickel is 8.50–9.50 %, yield strength is 590 MPa minimum and tensile strength is 690–830 MPa. It is the higher-strength 9 % nickel symbol and is used down to −196 °C, including LNG tanks, from 6 to 100 mm. Plate is supplied quenched and tempered; an intermediate treatment may be added. SHH STEEL produces and exports SL9N590 plate to the ordered edition, condition and dimensions.
Equivalent Grades:
Related 9 % nickel plates include GB/T 713.4 06Ni9DR and EN 10028-4 X8Ni9.
Heat Treatment
Quenched and tempered (JIS G 3127:2013).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is JIS G 3127 SL9N590 plate?

We produce and export JIS G 3127 SL9N590 as nickel steel plate for low-temperature pressure vessels and storage equipment. SL9N590 is a 9 % nickel grade with a heat-analysis nickel range of 8.50–9.50 %. Typical service includes cryogenic pressure vessels and LNG or liquid-nitrogen storage down to −196 °C, where the higher-strength quenched-and-tempered 9 % nickel symbol is specified.

JIS G 3127:2013 lists eight official symbols. This page specifies only SL9N590. Heat-treatment letters such as N, NT, TMC, TMCT, NNT and Q are marking symbols for the treatment actually given to the plate or test piece; they are not extra official kinds.

Composition, tensile properties, impact energy and heat-treatment conditions on this page follow JIS G 3127:2013. Specify the edition required on the purchase order.

SHH STEEL produces and exports JIS G 3127 SL9N590 plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for JIS G 3127 SL9N590

The items below follow JIS G 3127:2013. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard JIS G 3127:2013, Nickel steel plates for pressure vessels for low temperature services
Official symbol SL9N590
Product form Hot-rolled steel plate
How designations are listed Eight official symbols in JIS G 3127:2013 Table 1
Steelmaking Killed steel
Applicable thickness 6–100 mm (Table 1)
Minimum usable temperature listed in Table 1 −196 °C
Usual heat treatment Quenched and tempered. An intermediate heat treatment, cooling from the austenite-plus-ferrite two-phase region before tempering, may be added to improve toughness.
Heat-treatment marking Q (quenching and tempering). Test-piece symbols TN, TNT, T2NT and SR may be added when specimen heat treatment is ordered
Chemical analysis Heat analysis to JIS G 3127:2013 Table 3. Product analysis, when required, uses the permitted variations in JIS G 0321 Table 4
Tensile and bend properties JIS G 3127:2013 Table 4 (1 N/mm² = 1 MPa)
Impact properties JIS G 3127:2013 Table 5, Charpy V-notch, rolling direction unless otherwise agreed
Dimensions JIS G 3193, except thickness tolerances in JIS G 3127:2013 Table 6. Minus thickness tolerance is 0.25 mm unless a 0 mm minus tolerance is agreed
Appearance JIS G 3193 clause 7. Weld repair only with prior purchaser approval
Marking Official symbol and heat-treatment symbol, heat or inspection number, dimensions, and manufacturer name or abbreviation
Inspection document When no document type is named, JIS G 3127:2013 refers to JIS G 0415 inspection document 2.3 or inspection certificate 3.1.B
Our supply We produce and export SL9N590 plate to the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of JIS G 3127 SL9N590

JIS G 3127:2013 Table 3 is heat analysis. Other alloying elements may be added as needed; if they are added, their contents are reported on the inspection document.

Element SL9N590 heat analysis, JIS G 3127:2013 Table 3 (wt. %)
Carbon (C) 0.12 max
Silicon (Si) 0.30 max
Manganese (Mn) 0.90 max
Phosphorus (P) 0.015 max
Sulfur (S) 0.015 max
Nickel (Ni) 8.50–9.50

Tensile, bend and impact properties for JIS G 3127 SL9N590

JIS G 3127:2013 specifies tensile, bend and Charpy impact properties. Table 4 values are in N/mm², which the standard notes are equal to MPa.

Mechanical property (JIS G 3127:2013 Table 4) SL9N590
Yield strength or proof strength, MPa 590 min
Tensile strength, MPa 690–830
Elongation, % 21 min (No. 5 specimen, 6–16 mm. Table 4 also gives 25 % min (No. 5, over 16 mm) and 21 % min (No. 4, over 20 mm).)
Bend test 180°; inside radius 1.0× thickness at 19 mm and below, 1.5× thickness above 19 mm; No. 1 specimen; no crack on the outer surface

Charpy V-notch impact values below are JIS G 3127:2013 Table 5 at −196 °C. Transverse testing may be agreed; with purchaser approval the rolling-direction test may then be omitted.

Charpy V-notch (JIS G 3127:2013 Table 5) SL9N590
Test temperature, °C −196
Average of three 10×10 mm specimens, J 41 min
Individual 10×10 mm specimen, J 34 min
Subsize specimens For smaller specimens Table 5 requires averages of 21 J (10×5 mm) and 29 J (10×7.5 mm), with individual minima of 18 J and 25 J.

Delivery conditions for JIS G 3127 SL9N590

JIS G 3127:2013 Table 2 sets the heat treatment for SL9N590: Quenched and tempered. An intermediate heat treatment, cooling from the austenite-plus-ferrite two-phase region before tempering, may be added to improve toughness.

If the purchaser will heat-treat the plate, the plate may be supplied as-rolled by agreement, and the purchase order must state that fact and the heat-treatment conditions.

The usual marking addition for this treatment is Q (quenching and tempering). Examples in clause 4.5 include SL2N255N, SL3N275NT, SL3N255TMC, SL7N590TMCT, SL9N520NNT and SL9N590Q. Those suffixes record the treatment; they do not create extra official symbols beyond the eight kinds in Table 1.

The purchase order should name the official symbol, the heat-treatment symbol, thickness, width and length, any extra specimen heat treatment (including PWHT simulation, marked SR), and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

JIS G 3127:2013 does not specify a welding procedure. SL9N590 is a 9 % nickel pressure-vessel plate, not a general structural plate. Welding and thermal cutting should be qualified for the nickel content, thickness, delivery condition and the minimum temperature of the equipment.

Higher-nickel grades, especially the 9 % nickel symbols, are commonly welded with matching high-nickel filler metals and controlled heat input. Thermal cutting can harden the adjacent material; that zone should be considered, and removed where later forming or welding requires it.

Form, appearance, dimensions and thickness tolerances

Shape, dimensions, mass and most tolerances follow JIS G 3193. Length and cut-edge width tolerances are tolerance A unless otherwise specified. Thickness tolerances are JIS G 3127:2013 Table 6. The minus thickness tolerance is 0.25 mm; if a 0 mm minus tolerance is agreed, 0.25 mm is added to the plus side.

Appearance follows JIS G 3193 clause 7. Weld repair requires prior purchaser approval. Numeric thickness, width, length and flatness limits should be stated on the purchase order.

Applications and specification limits

We produce and export SL9N590 plate for cryogenic pressure vessels and LNG or liquid-nitrogen storage down to −196 °C, where the higher-strength quenched-and-tempered 9 % nickel symbol is specified. JIS G 3127:2013 Table 1 lists a minimum usable temperature of −196 °C for this symbol and an applicable thickness of 6–100 mm.

If the design temperature moves into a colder nickel class, or if a different official symbol, should be treated as a new material selection. Strength after a later heat treatment that is not the Table 2 condition is not assumed from the symbol alone.

JIS G 3127 is a nickel steel plate standard for low-temperature pressure vessels. It is not a carbon low-temperature plate standard such as JIS G 3126, and it is not an ASTM A353 or A553 order unless those specifications are written on the enquiry.

Compare JIS G 3127 SL9N590 with other steel plates

SL9N590 is a 9 % nickel low-temperature vessel plate. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
JIS G 3127 SL9N590 (this plate) 9 % nickel vessel plate, heat-analysis nickel 8.50–9.50 % Quenched and tempered. JIS G 3127:2013: yield 590 MPa minimum, tensile 690–830 MPa; Charpy average 41 J minimum at −196 °C on a 10×10 mm specimen Typical service includes cryogenic pressure vessels and LNG or liquid-nitrogen storage down to −196 °C, where the higher-strength quenched-and-tempered 9 % nickel symbol is specified A different nickel class, heat treatment or specification is not an automatic substitute
JIS G 3127 SL9N520 steel plate 9 % nickel vessel plate, heat-analysis nickel 8.50–9.50 % Double normalized and tempered. JIS G 3127:2013: yield 520 MPa minimum, tensile 690–830 MPa; Charpy average 34 J minimum at −196 °C on a 10×10 mm specimen Typical service includes cryogenic pressure vessels and storage equipment down to −196 °C, including LNG and liquid-nitrogen service, when the double-normalize-and-temper route is specified A different official symbol from SL9N590, not an automatic substitute
GB/T 713.4 06Ni9DR Chinese 9 % nickel cryogenic vessel plate Quenched and tempered Yield 560 MPa, tensile 680–820 MPa, service −196 °C LNG and other −196 °C vessel service Related 9 % nickel plate under a different specification, not an automatic substitute
EN 10028-4 X8Ni9 European 9 % nickel vessel plate, steel number 1.5662 As specified in EN 10028-4 490 MPa yield class, −196 °C service European 9 % nickel cryogenic vessels A different specification and yield class from this JIS symbol
ASME SA203 Grade E Nickel-alloy pressure-vessel plate in the normalized SA203 family. Normalized. Use its own ordered specification, thickness and delivery condition; no strength or toughness value is transferred to this grade. Low-temperature process vessels and refrigerated containment. Lower-nickel comparison, not a cryogenic-temperature substitute for JIS G3127 SL9N590 Steel Plate. Its Code edition, strength, impact temperature and certification must be selected separately.

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form before any substitution.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
Japan JIS G 3127:2013 SL9N590 This plate. Heat-analysis nickel 8.50–9.50 %, yield 590 MPa minimum, tensile 690–830 MPa, Charpy at −196 °C. Quenched and tempered. This product
China GB/T 713.4-2023 06Ni9DR A related 9 % nickel cryogenic vessel plate for −196 °C. Published yield is 560 MPa with tensile 680–820 MPa, against this symbol’s 590 MPa yield and 690–830 MPa tensile. Heat treatment for that designation is quenching and tempering. Related 9 % nickel plate under a different specification.
Europe EN 10028-4 X8Ni9 (1.5662) A related European 9 % nickel vessel plate for −196 °C. That designation is listed as a 490 MPa yield class, below both JIS 9 % nickel yield minima. Near name only.
United States ASTM A353 / A553 Type I Type I ASTM A553 Type I is the quenched-and-tempered 9 % nickel vessel plate; ASTM A353 uses a double-normalize-and-temper route. Nickel class and cryogenic purpose are related; tensile, impact and extra tests remain those of the named ASTM specification. Near names only. Dual marking only if both specifications are fully met.
International ISO 9328-1 and ISO 9328-4 No single ISO symbol specified JIS G 3127:2013 is based on ISO 9328-1:2011 and ISO 9328-4:2011 with modifications (MOD). The 2013 comparison notes that JIS lists eight kinds and treats SL7N590 as its own kind. Use the JIS symbol on the order unless an ISO designation is separately specified.

Why choose SHH STEEL for JIS G 3127 SL9N590

  • We produce and export JIS G 3127 SL9N590 nickel steel plate
  • We review the enquiry for edition, symbol, heat-treatment mark, dimensions and extra tests
  • We keep the eight official symbols distinct, including the N, Q and NNT delivery routes
  • We match documentation to what the purchase order requires

How to enquire for JIS G 3127 SL9N590 plate

Item What to specify
Standard and symbol JIS G 3127 SL9N590 and the edition required
Heat-treatment mark Q (quenching and tempering)
Dimensions Required thickness (6–100 mm in Table 1), width and length
Chemistry Heat analysis to JIS G 3127:2013 Table 3, or to another edition if specified
Mechanical tests Tensile and bend properties to Table 4; Charpy tests to Table 5 unless a lower test temperature is agreed
Other tests Ultrasonic examination or other extra tests only when written on the order
Documentation State the inspection document type required by the project
Processing Cutting or other processing only when requested

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Does JIS G 3127 cover only 9 % nickel plate?
No. JIS G 3127:2013 lists eight official symbols: SL2N255, SL3N255, SL3N275, SL3N440, SL5N590, SL7N590, SL9N520 and SL9N590. This page is SL9N590.
Which edition do the tables on this page follow?
They follow JIS G 3127:2013. Specify the edition required on the purchase order.
What do suffixes such as N, Q or NNT mean?
They are official heat-treatment marking symbols in JIS G 3127:2013 clause 4.5, not extra kinds. For SL9N590 the usual mark is Q (quenching and tempering). Test-piece letters such as SR can be added when specimen heat treatment is ordered.
Can another nickel vessel plate be used in place of SL9N590?
Only after a project review. Related names in other specifications may share a nickel class but differ in yield, tensile range, heat treatment or impact temperature.
What should a quotation enquiry include?
JIS G 3127 SL9N590, the edition required, the heat-treatment mark, plate thickness by width by length, quantity, any extra tests or specimen heat treatment, and the inspection document required by the project.

Request a quotation

Contact SHH STEEL for a quotation for JIS G 3127 SL9N590 nickel steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the heat-treatment condition and marking symbol, and say if specimen heat treatment or a PWHT simulation is required. If your project requires a stated impact temperature below the Table 5 value, ultrasonic examination or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X