JIS G 3106 SM490 Equal and Unequal Steel Angles | JIS G 3106 Steel Angles - SHH STEEL

JIS G 3106 SM490 Equal and Unequal Steel Angles

JIS G 3106 SM490 steel angle is a Japanese welded-structure angle in the 490–610 N/mm² tensile class. The page covers SM490A, B, C, YA and YB, lists the JIS G 3192 equal, unequal and unequal-thickness series, and gives heat analysis, yield tables and the 0 °C impact rules that apply above 12 mm.
Keywords
JIS G 3106 SM490 Steel Angle, SM490 angle, SM490B angle, JIS G 3192 angle, SM490C
Equivalent Grades:
SM490 H-beam (same material family); SS400 angle (same shape series, general-structure grade); Q355B angle; S355JR — comparisons only, not automatic substitutes.
Share:
General Description
Material Specification
Available Sizes of JIS G 3106 SM490 Equal Leg Steel Angles
Available Sizes of JIS G 3106 SM490 Unequal Leg Steel Angles
Chemical Composition of SM490 Steel Angle
Mechanical Properties of SM490 Steel Angle
Delivery Conditions, Inspection and Identification
Weldability of SM490 Steel Angles
Shape Tolerances and Theoretical Mass
Applications and Service Limits
SM490 Compared with SS400, Q355B and S355JR
Near-Equivalents: Not Automatic Substitutes
Sourcing SM490 Steel Angles from SHH STEEL
FAQ
Conclusion

What is JIS G 3106 SM490 Steel Angle?

JIS G 3106 SM490 steel angle is a hot-rolled Japanese angle whose material grade is one of the SM490 qualities under JIS G 3106 — SM490A, SM490B, SM490C, SM490YA or SM490YB — and whose shape, mass and tolerances are ordered to JIS G 3192 Tables 8, 9 and 10. SM stands for rolled steel for welded structure, and 490 is the tensile-strength class (490–610 N/mm²). There is no suffixless grade in the standard called only “SM490”; the quality letter must be named on the order.

This page covers the SM490 family in angle form. The H-section sister is JIS G 3106 SM490 H-beam. A general-structure comparison on the same angle series is JIS G 3101 SS400 steel angle.

These bars are filed under steel angle profiles in the steel structural profiles category. The designation is the leg and thickness string itself: A×A×t, A×B×t or A×B×t1×t2, for example 75×75×9, 150×100×12 or 200×90×9×14. JIS G 3192 does not require an ASTM-style L prefix. A 75 mm Japanese equal angle is not a European EN 10056 L 75×75, an American L, or a Chinese GB/T 706 angle of similar millimetre size.

This page covers Equal and Unequal Steel Angles in JIS G 3106 SM490. The Equal Leg Steel Angles (JIS G 3192 Table 8) and Unequal Leg Steel Angles (Tables 9 and 10) follow JIS G 3192; the material standard does not by itself define the dimensions.

Material, Dimensions and the SM490 Quality Family

The purchase order and the inspection document should name, separately:

  • JIS G 3106 and its edition (this page uses the 2020 edition as the numeric basis; the edition named on the order governs), and the full quality symbol SM490A, SM490B, SM490C, SM490YA or SM490YB;
  • the JIS G 3192 designation (A×A×t, A×B×t or A×B×t1×t2);
  • any agreed heat-treatment suffix and any agreed Ceq or PCM limit.
Symbol Standard scope for sections (mm) Heat-analysis carbon, max (%) Charpy requirement in JIS G 3106:2020 (thickness > 12 mm)
SM490A ≤ 200 0.20 (t ≤ 50); 0.22 (50 < t ≤ 200) Not listed in Table 8. No standard impact test; do not infer one from the 490 tensile class.
SM490B ≤ 200 0.18 (t ≤ 50); 0.20 (50 < t ≤ 200) 27 J at 0 °C, V-notch, rolling direction.
SM490C ≤ 100 0.18 (t ≤ 100) 47 J at 0 °C, V-notch, rolling direction. This is not the same energy as SM490B.
SM490YA ≤ 100 0.20 (t ≤ 100) Not listed in Table 8. Higher yield than A/B/C, but still no standard impact test.
SM490YB ≤ 100 0.20 (t ≤ 100) 27 J at 0 °C, V-notch, rolling direction, with the higher YA/YB yield table.

JIS G 3106 SM490 Equal Leg Steel Angles

The tables are the complete tabulated standard series in JIS G 3192:2024: Table 8 equal-leg (40 sizes, 25×25×3 to 250×250×35), Table 9 unequal-leg (13 sizes, 90×75×9 to 150×100×15), and Table 10 unequal-leg unequal-thickness (7 sizes, 200×90×9×14 to 400×100×13×18). The tabulated dimensions are representative; other section dimensions may be used by agreement. Table 10 is a distinct series and is not mixed into Table 9. Not every mill rolls every designation in every SM490 quality.

Equal-leg angles (Table 8)

Swipe horizontally to view all dimensions.

Designation (A×A×t) A (mm) t (mm) r1 (mm) r2 (mm) Area (cm²) Mass (kg/m)
25×25×3 25 3 4 2 1.427 1.12
30×30×3 30 3 4 2 1.727 1.36
40×40×3 40 3 4.5 2 2.336 1.83
40×40×5 40 5 4.5 3 3.755 2.95
45×45×4 45 4 6.5 3 3.492 2.74
45×45×5 45 5 6.5 3 4.302 3.38
50×50×4 50 4 6.5 3 3.892 3.06
50×50×5 50 5 6.5 3 4.802 3.77
50×50×6 50 6 6.5 4.5 5.644 4.43
60×60×4 60 4 6.5 3 4.692 3.68
60×60×5 60 5 6.5 3 5.802 4.55
65×65×5 65 5 8.5 3 6.367 5.00
65×65×6 65 6 8.5 4 7.527 5.91
65×65×8 65 8 8.5 6 9.761 7.66
70×70×6 70 6 8.5 4 8.127 6.38
75×75×6 75 6 8.5 4 8.727 6.85
75×75×9 75 9 8.5 6 12.69 9.96
75×75×12 75 12 8.5 6 16.56 13.0
80×80×6 80 6 8.5 4 9.327 7.32
90×90×6 90 6 10 5 10.55 8.28
90×90×7 90 7 10 5 12.22 9.59
90×90×10 90 10 10 7 17.00 13.3
90×90×13 90 13 10 7 21.71 17.0
100×100×7 100 7 10 5 13.62 10.7
100×100×10 100 10 10 7 19.00 14.9
100×100×13 100 13 10 7 24.31 19.1
120×120×8 120 8 12 5 18.76 14.7
130×130×9 130 9 12 6 22.74 17.9
130×130×12 130 12 12 8.5 29.76 23.4
130×130×15 130 15 12 8.5 36.75 28.8
150×150×12 150 12 14 7 34.77 27.3
150×150×15 150 15 14 10 42.74 33.6
150×150×19 150 19 14 10 53.38 41.9
175×175×12 175 12 15 11 40.52 31.8
175×175×15 175 15 15 11 50.21 39.4
200×200×15 200 15 17 12 57.75 45.3
200×200×20 200 20 17 12 76.00 59.7
200×200×25 200 25 17 12 93.75 73.6
250×250×25 250 25 24 12 119.4 93.7
250×250×35 250 35 24 18 162.6 128

JIS G 3106 SM490 Unequal Leg Steel Angles

Unequal-leg angles (Table 9)

Swipe horizontally to view all dimensions.

Designation (A×B×t) A (mm) B (mm) t (mm) r1 (mm) r2 (mm) Area (cm²) Mass (kg/m)
90×75×9 90 75 9 8.5 6 14.04 11.0
100×75×7 100 75 7 10 5 11.87 9.32
100×75×10 100 75 10 10 7 16.50 13.0
125×75×7 125 75 7 10 5 13.62 10.7
125×75×10 125 75 10 10 7 19.00 14.9
125×75×13 125 75 13 10 7 24.31 19.1
125×90×10 125 90 10 10 7 20.50 16.1
125×90×13 125 90 13 10 7 26.26 20.6
150×90×9 150 90 9 12 6 20.94 16.4
150×90×12 150 90 12 12 8.5 27.36 21.5
150×100×9 150 100 9 12 6 21.84 17.1
150×100×12 150 100 12 12 8.5 28.56 22.4
150×100×15 150 100 15 12 8.5 35.25 27.7

Unequal-leg unequal-thickness angles (Table 10)

Swipe horizontally to view all dimensions.

Designation (A×B×t1×t2) A (mm) B (mm) t1 (mm) t2 (mm) r1 (mm) r2 (mm) Area (cm²) Mass (kg/m)
200×90×9×14 200 90 9 14 14 7 29.66 23.3
250×90×10×15 250 90 10 15 17 8.5 37.47 29.4
250×90×12×16 250 90 12 16 17 8.5 42.95 33.7
300×90×11×16 300 90 11 16 19 9.5 46.22 36.3
300×90×13×17 300 90 13 17 19 9.5 52.67 41.3
350×100×12×17 350 100 12 17 22 11 57.74 45.3
400×100×13×18 400 100 13 18 24 12 68.59 53.8

SM490 Chemical Composition (Heat Analysis)

The figures below are heat-analysis maxima from JIS G 3106:2020 Table 2. For these angles the relevant thickness is that at the test-piece location, ordinarily the leg thickness t, or the thicker leg t2 on the Table 10 series, not the leg length A or B.

Symbol Thickness (mm) C max Si max Mn max P max S max
SM490A t ≤ 50 0.20 0.55 1.65 0.035 0.035
SM490A 50 < t ≤ 200 0.22 0.55 1.65 0.035 0.035
SM490B t ≤ 50 0.18 0.55 1.65 0.035 0.035
SM490B 50 < t ≤ 200 0.20 0.55 1.65 0.035 0.035
SM490C t ≤ 100 0.18 0.55 1.65 0.035 0.035
SM490YA / SM490YB t ≤ 100 0.20 0.55 1.65 0.035 0.035

Several of the larger tabulated equal-leg sizes have a leg thicker than 16 mm, and some exceed 40 mm or 50 mm, so later carbon and yield bands do apply when the leg is the test location. Clause 7.2 Ceq and PCM tables apply to plates and sheets manufactured by a thermo-mechanical control process. They are not a default as-rolled angle CEV. If a Ceq or PCM limit is required on a section order, it must be agreed and stated on the certificate; no value is invented here.

SM490 Mechanical Properties: Yield, Tensile and 0 °C Impact

Tensile properties follow Table 7 of JIS G 3106:2020. Thickness is that at the location of the test pieces, ordinarily the leg t, or the thicker leg t2 on Table 10. Do not read the first yield band against the longer leg length. Annex JB of JIS G 3106 applies only to sections whose leg length is under 40 mm: in Table 8, only the 25×25 and 30×30 families. Review those bars against Annex JB in the edition named on the order; the numeric JB values are not restated here. Annex JB does not apply to the 40×40 family or to any Table 9 or Table 10 size.

Thickness at the test-piece location (mm) Min. yield, SM490A/B/C (N/mm²) Tensile strength (N/mm²)
t ≤ 16 325 490–610
16 < t ≤ 40 315 490–610
40 < t ≤ 75 295 490–610
75 < t ≤ 100 295 490–610
100 < t ≤ 160 285 (A and B only) 490–610 (A and B only)
160 < t ≤ 200 275 (A and B only) 490–610 (A and B only)

SM490YA and SM490YB use a higher yield table, still in the 490–610 N/mm² tensile class, with a standard section scope of 100 mm or less:

Thickness at the test-piece location (mm) Min. yield, SM490YA/YB (N/mm²) Tensile strength (N/mm²)
t ≤ 16 365 490–610
16 < t ≤ 40 355 490–610
40 < t ≤ 75 335 490–610
75 < t ≤ 100 325 490–610

Elongation is as follows:

Thickness (mm) Test piece Min. elongation, A/B/C (%) Min. elongation, YA/YB (%)
t ≤ 5 No. 5 22 19
5 < t ≤ 16 No. 1A 17 15
16 < t ≤ 50 No. 1A 21 19
t > 40 No. 4 23 21

When impact testing applies (the symbols listed in Table 8, with thickness over 12 mm), the requirements are:

Symbol Test temperature (°C) Minimum absorbed energy (J) Test piece and direction
SM490A — Not specified in Table 8 —
SM490B 0 27 V-notch, rolling direction
SM490C 0 47 V-notch, rolling direction
SM490YA — Not specified in Table 8 —
SM490YB 0 27 V-notch, rolling direction

A lower test temperature may be agreed. An A or YA certificate does not demonstrate a 0 °C test. Some of the smaller tabulated legs are 12 mm or thinner; clause 8.2 is written for thickness over 12 mm.

Delivery Conditions, Inspection and Identification

SM490 angles are commonly supplied as-rolled. Heat treatment is used when agreed; any agreed suffix is added to the quality symbol. The inspection document should identify JIS G 3106 and its edition, the full quality symbol, the JIS G 3192 designation, heat analysis, and tensile results against the thickness at the test location, plus the Table 8 impact result for B, C or YB when that test applies. A plate, H-beam or channel certificate does not, by itself, identify an angle.

Weldability of SM490 Steel Angles

SM490 is specified as a weldable rolled steel for welded structures. Preheat and consumable choice should use the certified heat analysis, any agreed Ceq or PCM, the actual thickness and the joint design. A CEV figure must not be read off a TMCP plate table as if it automatically applied to an as-rolled angle.

JIS G 3192 Shape Tolerances and Theoretical Mass

Shape, mass and tolerances belong to the ordered edition of JIS G 3192. Mass in the size table is the published theoretical figure. Millimetre tolerance tables are not reproduced here. Settlement on theoretical or weighed mass should follow the contract.

Applications and Service Limits

SM490 angles are used in welded frames, bracing and similar work where a Japanese welded-structure grade in the 490 N/mm² tensile class is named. Choose the quality letter for the impact or yield table actually required. They are not a silent substitute for JIS G 3101 SS400 steel angle, for a GB/T 706 angle, or for a European L section in S355JR.

SM490 Compared with SS400, Q355B and S355JR

The comparisons below are an orientation only; they are not automatic substitutes.

Grade / designation Standard Relationship to SM490 angle Caution
SM490 H-beam JIS G 3106; dimensions JIS G 3192 Table 15 The same material family in H-section form. An angle designation is not an H-section. See JIS G 3106 SM490 H-beam.
SS400 angle JIS G 3101; dimensions JIS G 3192 Tables 8, 9 and 10 A general-structure comparison on the same angle series, at a lower tensile class and with no Charpy table. SS400 is not a welded-structure SM grade. See JIS G 3101 SS400 steel angle.
Q355B angle GB/T 1591; dimensions GB/T 706 A Chinese 355 MPa angle often compared with the SM490 tensile class. The GB/T 706 designation is not a JIS A×A×t string. See GB/T 706 Q355B steel angle.
S355JR EN 10025-2; dimensions EN 10056 A European 355 MPa comparison, usually as equal or unequal L sections. JR, J0 and J2 are different impact qualities, and the shape systems differ.

Near-Equivalents: Not Automatic Substitutes

A near-equivalent is a starting point for a discussion, not a licence to swap certificates. If a project names SM490B or SM490C, keep that quality letter and JIS G 3192 on the order. The H-section sister is JIS G 3106 SM490 H-beam.

Sourcing SM490 Steel Angles from SHH STEEL

SHH STEEL supplies JIS G 3106 SM490 steel angles against a named designation list, the quality letter, the material edition and the inspection document type. Enquiries should state the A×A×t, A×B×t or A×B×t1×t2 designations, the quality (A, B, C, YA or YB), cut lengths or mill lengths, any processing, and whether JIS G 3101 SS400 steel angle is acceptable on part of the list.

The size table is the standard series, not a claim that every designation is rolled in every quality. Once the list is clear, a quotation can be prepared against the stated edition and certificate.

SM490 Steel Angle FAQs

Is there a single grade called just SM490?
No. The standard uses SM490A, SM490B, SM490C, SM490YA and SM490YB. A and YA have no standard Table 8 impact test. B and YB require 27 J at 0 °C when testing applies; C requires 47 J at 0 °C. YA and YB use a higher yield table.
Which thickness is used for yield and impact on an angle?
Thickness is that at the location of the test pieces, ordinarily the leg t, or the thicker leg t2 on the Table 10 series, not the leg length. Impact testing, when it applies, is written for thickness over 12 mm.
Does Annex JB apply to every small SM490 angle?
Annex JB of JIS G 3106 applies only to sections whose leg length is under 40 mm. In the Table 8 series that means only the 25×25 and 30×30 families. It does not apply to 40×40 or to any Table 9 or Table 10 size. This page does not restate the numeric JB values.
Which edition of JIS G 3106 is used on this page?
The numeric tables use JIS G 3106:2020. Dimensional sizes use JIS G 3192:2024 Tables 8, 9 and 10. A later edition of either standard may be named on the order; the ordered edition governs.

Request a Quotation for JIS G 3106 SM490 Steel Angle

JIS G 3106 SM490 steel angle is a welded-structure angle in the 490–610 N/mm² tensile class. Nominate the JIS G 3192 designation (A×A×t, A×B×t or A×B×t1×t2), the quality letter (A, B, C, YA or YB), JIS G 3106:2020 or the edition on the order, and the inspection document type. Send the size list, quality, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X