GB/T 19189 07MnNiMoDR Steel Plate | 07MnNiMoDR -50°C QT Vessel Plate (Now Q490DRL2)
What is GB/T 19189-2011 07MnNiMoDR steel plate?
GB/T 19189 07MnNiMoDR Steel Plate is low weld-crack-sensitivity Mn-Ni-Mo steel for low-temperature vessels, supplied quenched and tempered for welded pressure vessels under GB/T 19189-2011. The suffix R stands for pressure vessel (rong) and D for low temperature (di) in the Chinese designation system; the leading 07 or 12 indicates the nominal carbon level.
GB/T 19189-2011, Quenched and tempered high strength steel plates for pressure vessels, was issued on 16 June 2011 (as GB 19189-2011) and implemented on 1 February 2012, replacing the 2003 edition. It has since been fully replaced by GB/T 713.6-2023, Steel plate, sheet and strip for pressure equipment – Part 6: Quenched and tempered high strength steel, implemented on 1 March 2024. GB/T 19189-2011 is therefore a superseded standard and is not the current Chinese specification for this plate.
The documented successor of 07MnNiMoDR is GB/T 713.6 Q490DRL2 Steel Plate: the GB/T 150-2024 errata replace the material 07MnNiMoDR / GB/T 19189 with Q490DRL2 / GB/T 713.6 in the vessel code tables. The 2023 book renamed the grades by yield strength and changed the phosphorus and sulfur maxima, so the two are related designations, not the same specification. New designs should be ordered to GB/T 713.6-2023; this page is for drawings, data sheets and replacement records that still call for GB/T 19189-2011.
SHH STEEL produces and exports 07MnNiMoDR plate to the edition, thickness, impact and inspection requirements written on the enquiry. The grade sits in our GB/T 19189 range under Boiler & Pressure Vessel Steel Plates.
Material specification for GB/T 19189 07MnNiMoDR
The items below follow GB/T 19189-2011. Thickness, width, length and inspection document are confirmed against the enquiry rather than listed as stock ranges.
| Parameter | Detail |
|---|---|
| Standard | GB/T 19189-2011 (issued as GB 19189-2011), Quenched and tempered high strength steel plates for pressure vessels |
| Edition status | Superseded. Fully replaced by GB/T 713.6-2023 (implemented 1 March 2024). This page covers the 2011 edition only |
| Successor designation | Q490DRL2 in GB/T 713.6-2023 (GB/T 150-2024 errata) |
| Grades in the 2011 edition | 07MnMoVR, 07MnNiVDR, 07MnNiMoDR, 12MnNiVR |
| Grade | 07MnNiMoDR |
| Previous designation | This grade was added in the 2011 edition; it had no 2003 predecessor. |
| Scope of the standard | Plates 10 mm to 60 mm thick for pressure vessels |
| Thickness tabulated for this grade | 10–50 mm (Table 2 limit, not a stock range) |
| Steelmaking | Basic oxygen or electric furnace, with vacuum treatment |
| Delivery condition | Quenched and tempered; tempering temperature not below 600°C; edges sheared or flame cut |
| Impact requirement | Charpy V, transverse, -50°C, KV2 ≥80 J |
| Ultrasonic testing | Every plate, JB/T 4730.3 or GB/T 2970, acceptance level I |
| Dimensions and tolerances | GB/T 709, thickness tolerance Class B; Class C by agreement; theoretical weight on mean thickness, density 7.85 g/cm³ |
| Related standard | Not equivalent (NEQ) to JIS G3115-2005, per the foreword |
Chemical composition of GB/T 19189-2011 07MnNiMoDR
The heat analysis below is the 07MnNiMoDR row of GB/T 19189-2011 Table 1. Pcm is the weld crack sensitivity composition, Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B (%).
| Element | Heat analysis, GB/T 19189-2011 Table 1 (wt. %) |
|---|---|
| Carbon (C) | ≤0.09 |
| Silicon (Si) | 0.15–0.40 |
| Manganese (Mn) | 1.20–1.60 |
| Phosphorus (P) | ≤0.015 |
| Sulfur (S) | ≤0.005 |
| Copper (Cu) | ≤0.25 |
| Nickel (Ni) | 0.30–0.60 |
| Chromium (Cr) | ≤0.30 |
| Molybdenum (Mo) | 0.10–0.30 |
| Vanadium (V) | ≤0.06 |
| Boron (B) | ≤0.0020 |
| Pcm (weld crack sensitivity) | ≤0.21 |
Clause 6.1.3 removes the molybdenum lower limit for 07MnNiMoDR plate not thicker than 30 mm. This grade has the tightest phosphorus and sulfur limits of the four. Micro-alloying elements other than those listed may be added to improve properties (clause 6.1.2). Product analysis tolerances follow GB/T 222, with phosphorus +0.003 % and sulfur +0.002 % (clause 6.1.4).
These are 2011 values. GB/T 713.6-2023 changed the phosphorus and sulfur maxima, so the 2011 row must not be used as a Q490DRL2 chemistry, and the Q490DRL2 table must not be used for a 2011 order.
Mechanical properties of GB/T 19189-2011 07MnNiMoDR
Table 2 of GB/T 19189-2011 sets one property band for 07MnNiMoDR across its thickness range.
| Nominal thickness (mm) | Yield strength ReL, min (MPa) | Tensile strength Rm (MPa) | Elongation A, min (%) | Charpy V test temperature | KV2, min (J) | 180° bend, b = 2a |
|---|---|---|---|---|---|---|
| 10–50 | 490 | 610–730 | 17 | -50°C | 80 | d = 3a |
Where yield is not distinct, Rp0.2 is used. Charpy energy is the mean of three specimens; one value may be below the Table 2 figure but not below 70 % of it. Plate under 12 mm is tested with 7.5 × 10 × 55 mm sub-size specimens, with results not less than 75 % of the Table 2 value. By agreement, plate over 36 mm may receive an extra impact set at mid-thickness, with the energy agreed between the parties (clause 6.4.4).
If an impact result fails, three more specimens are taken from the same plate; the mean of all six must meet the requirement, no more than two may be below it, and only one may be below 70 % of it.
Delivery conditions for GB/T 19189 07MnNiMoDR
Plates are delivered in the quenched-and-tempered condition, with tempering at not less than 600°C, and are cut by shearing or flame cutting. As-rolled, normalized or TMCP plate is not a GB/T 19189-2011 delivery condition.
The mechanical values apply to the QT condition supplied. If the vessel will receive post-weld heat treatment, the PWHT cycle and any simulated PWHT testing should be written on the order, because PWHT can lower strength in QT steels.
Welding and thermal cutting
07MnNiMoDR is one of the three low weld-crack-sensitivity grades of the 2011 book. The Pcm ceiling in Table 1 limits the hardenability that drives hydrogen cracking, which helps reduce preheat on thick QT plate.
Preheat, interpass temperature, heat input and any PWHT are set by the qualified procedure, the thickness and the vessel code, not by the grade name. Excessive heat input can soften or embrittle the HAZ of QT steel, so procedures should be qualified with impact tests at the vessel test temperature.
Dimensions, tolerances and inspection
Dimensions, shape and permitted deviations follow GB/T 709; thickness tolerance is Class B unless Class C is agreed. Plates are invoiced on theoretical weight using the mean of the maximum and minimum permitted thickness.
Cracks, blisters, scabs, folds, inclusions and laminations are not permitted. Surface defects may be dressed to a depth of not more than half the thickness tolerance, keeping the minimum thickness, with smooth dressed areas.
Each heat-treated plate is inspected as its own batch. Per heat: one chemical analysis. Per batch: one tensile, three Charpy and one bend specimen, all transverse, taken at quarter width; plates longer than 15 m after heat treatment are sampled at both ends. For plate over 25 mm the impact specimen axis is at quarter thickness. Every plate is ultrasonically tested to level I.
Applications and specification limits
We produce and export 07MnNiMoDR for low-temperature vessels where the design accepts a -50°C impact test, such as spherical tanks and large storage vessels where the 490 MPa yield class allows thinner walls than conventional carbon-manganese plate. The minimum design temperature is set by the vessel code, the thickness and the impact test, not by the grade name.
The other grades of the 2011 book are GB/T 19189 07MnMoVR Steel Plate, GB/T 19189 07MnNiVDR Steel Plate, GB/T 19189 12MnNiVR Steel Plate. They differ in impact temperature, alloy route and welding purpose and are not interchangeable without design review.
Edition note. This page is the GB/T 19189-2011 product. New designs should use GB/T 713.6 Q490DRL2 Steel Plate under GB/T 713.6-2023. A certificate to one edition is not an automatic substitute for an order written to the other.
GB/T 19189-2011 is a pressure vessel plate standard. On its own it does not impose supplementary special-code requirements; where such a code applies, its supplementary requirements must be written on the order.
Compare GB/T 19189 07MnNiMoDR with other QT vessel plates
The comparison below places 07MnNiMoDR against its 2011 siblings, its 2023 successor and familiar foreign QT vessel plates. They are related by service, not interchangeable.
| Material | Type | Delivery | Key requirement | Substitution limit |
|---|---|---|---|---|
| GB/T 19189 07MnNiMoDR (this plate) | Mn-Ni-Mo, low Pcm, lowest test temperature | QT | ReL 490 MPa min; -50°C / 80 J; 10–50 mm | 2011 edition only |
| GB/T 19189 07MnMoVR Steel Plate | Mn-Mo-V, low Pcm | QT | ReL 490 MPa min; -20°C / 80 J; 10–60 mm | Different impact class or welding purpose |
| GB/T 19189 07MnNiVDR Steel Plate | Mn-Ni-V, low Pcm, low-temperature | QT | ReL 490 MPa min; -40°C / 80 J; 10–60 mm | Different impact class or welding purpose |
| GB/T 19189 12MnNiVR Steel Plate | Mn-Ni-V, high heat-input welding | QT | ReL 490 MPa min; -20°C / 80 J; 10–60 mm | Different impact class or welding purpose |
| GB/T 713.6 Q490DRL2 Steel Plate | 2023 successor designation | QT | 2023 tables; see that page | Successor, not the same specification |
| JIS G3115 SPV490 Steel Plate | JIS QT vessel plate, 490 class | QT | Per JIS G3115 | Related; the 2011 foreword marks JIS G3115-2005 as not equivalent (NEQ) |
| EN 10028-6 P460QL2 Steel Plate | QT fine-grain vessel plate, 460 MPa yield class, low-temperature L2 quality | QT | Per EN 10028-6 | Different strength and impact system; related by service only |
Equivalent and related grades by country
The designations below are related grades by product type and service, not certified equivalents. Strength, impact temperature, thickness limits, chemistry and delivery condition must be checked against the project specification before any substitution.
| Country / region | Standard | Grade | Similarity and key differences | Caveat |
|---|---|---|---|---|
| China | GB/T 19189-2011 | 07MnNiMoDR | This product | Superseded edition |
| China | GB/T 713.6-2023 | GB/T 713.6 Q490DRL2 Steel Plate | Documented successor designation (GB/T 150-2024 errata) | Revised P/S limits and tables; not automatic |
| China | GB 19189-2003 | — | This grade was added in the 2011 edition; it had no 2003 predecessor. | Withdrawn earlier edition; for record matching only |
| Japan | JIS G3115 | JIS G3115 SPV490 Steel Plate | QT pressure vessel plate in the 490 class | 2011 foreword: NEQ to JIS G3115-2005 |
| Europe | EN 10028-6 | EN 10028-6 P460QL2 Steel Plate | QT fine-grain vessel plate, 460 MPa yield class, low-temperature L2 quality | 460 vs 490 MPa yield class; different impact rules |
| United States | ASTM A537 | ASTM A537 Class 2 Steel Plate | Quenched-and-tempered C-Mn-Si vessel plate | Lower strength class; impact only as specified; related only |
Why choose SHH STEEL for GB/T 19189 07MnNiMoDR
- SHH STEEL produces and exports GB/T 19189-2011 07MnNiMoDR plate as a producer, exporter and mill agent
- We quote to the edition written on your order and keep 2011 values separate from GB/T 713.6 Q490DRL2 values
- We check that the -50°C impact class and the 10–50 mm thickness limit match the design before quoting
- We review tempering, ultrasonic level, mid-thickness impact and simulated PWHT requirements before rolling, not after
- We match the inspection document to what the purchase order requires
How to enquire for GB/T 19189 07MnNiMoDR plate
| Item | What to specify |
|---|---|
| Standard and grade | GB/T 19189-2011 07MnNiMoDR; state the edition year. If the design allows, consider GB/T 713.6-2023 Q490DRL2 |
| Dimensions | Thickness (10–50 mm in Table 2), width and length; we confirm production and export feasibility against the enquiry |
| Impact testing | -50°C / 80 J per Table 2; state any mid-thickness set for plate over 36 mm |
| Heat treatment | QT with tempering not below 600°C; state the PWHT cycle and any simulated PWHT |
| Ultrasonic testing | Every plate to JB/T 4730.3 or GB/T 2970, level I, or a stricter agreed requirement |
| Documentation | Inspection document type required by the project, for example EN 10204 3.1 or 3.2 |
| Other editions | If GB/T 713.6-2023 must also be met, say so; we review both editions before quoting |
FAQ
-
Is GB/T 19189-2011 still the current standard for 07MnNiMoDR?
- No. GB/T 19189-2011 has been fully replaced by GB/T 713.6-2023, implemented on 1 March 2024, where the corresponding designation is Q490DRL2. We still produce 07MnNiMoDR to the 2011 edition when the purchase documents require it.
-
What replaced 07MnNiMoDR?
- The GB/T 150-2024 errata replace 07MnNiMoDR / GB/T 19189 with Q490DRL2 / GB/T 713.6 in the vessel code tables. The 2023 book has revised chemistry limits, so the two are not identical specifications.
-
What are the mechanical properties of 07MnNiMoDR?
- GB/T 19189-2011 Table 2 requires ReL ≥490 MPa, Rm 610–730 MPa, A ≥17 %, 80 J Charpy at -50°C and a 180° bend at d = 3a for 10–50 mm plate.
-
How is 07MnNiMoDR delivered?
- Quenched and tempered with tempering at not less than 600°C, vacuum-treated steel, every plate ultrasonically tested to level I.
-
What should a quotation enquiry include?
- GB/T 19189-2011, grade 07MnNiMoDR, thickness by width by length, quantity, impact and ultrasonic requirements, PWHT or simulated PWHT, and the inspection document.
Request a quotation
Contact SHH STEEL for a quotation for GB/T 19189-2011 07MnNiMoDR quenched-and-tempered pressure vessel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.
State the Charpy requirement if it differs from Table 2, any mid-thickness impact set, the ultrasonic standard and level, the PWHT or simulated PWHT cycle, and the inspection document required by the project.
If you are considering GB/T 713.6-2023 Q490DRL2 or another 2011 grade, send the design temperature and project specification with your enquiry. We will review the differences rather than assume the grades or editions are interchangeable.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.
Contact: admin@steelspecs.com