GB/T 11251 20Cr Alloy Steel Plate
What is GB/T 11251 Grade 20Cr plate?
GB/T 11251 20Cr Alloy Steel Plate is alloy structural steel plate and strip purchased to GB/T 11251-2025. Grade 20Cr is one of the fourteen grades for which the 2025 edition publishes annealed single-rolled tensile and elongation values in Table 1. It is a chromium engineering grade, not 20CrMo and not a vessel-plate R-suffix steel.
The 2025 edition is a plate and strip book. Chemical composition shall comply with GB/T 3077, used here as the chemistry reference, not as the delivery book.
Single-rolled plate is usually supplied high-temperature tempered unless another condition is agreed. Parts cut from 20Cr plate are often carburized later. That later case-hardening cycle is not an automatic GB/T 11251 as-delivered guarantee.
SHH STEEL produces and exports GB/T 11251-2025 Grade 20Cr plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry. This grade belongs to our Alloy Steel Plates range under GB/T 11251.
Material specification for GB/T 11251 Grade 20Cr
The items below follow GB/T 11251-2025. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.
| Parameter | Detail |
|---|---|
| Standard | GB/T 11251-2025, Alloy structural steel plate, sheet and strip. Published 31 October 2025 and implemented 1 May 2026. It replaces GB/T 11251-2020 and GB/T 37601-2019 |
| Grade designation | Grade 20Cr, chromium alloy structural steel plate listed in GB/T 11251-2025 Table 1 |
| Product forms in the standard | Single-rolled hot-rolled plate, nominal thickness 3.0 mm to 250 mm; and continuous-rolled plate and strip, nominal thickness not greater than 25.4 mm (wide strip and cut plate or slit strip 600 mm wide or more, and narrow strip and cut plate under 600 mm) |
| Chemical composition | Shall comply with GB/T 3077. Optional phosphorus or sulfur variants may be agreed under clause 6.1.1. Product analysis shall meet GB/T 222 |
| Single-rolled delivery | High-temperature tempered as the usual condition; annealed, normalized, normalized and tempered, or quenched and tempered by agreement. Normalizing rolling may replace normalizing if the normalized mechanical requirements can be met |
| Continuous-rolled delivery | As-rolled; heat treatment by agreement. If spheroidize-annealed, surface hardness shall meet GB/T 3077. Tensile tests on continuous-rolled material are by agreement |
| Annealed single-rolled mechanics | Table 1 applies to Grade 20Cr at nominal thickness not greater than 100 mm. Thickness over 100 mm, and grades other than Table 1, are by agreement |
| Dimensions | Single-rolled plate to GB/T 709-2019, thickness tolerance class A. Wide strip and cut plate or slit strip to GB/T 709-2019 Table 4 thickness tolerances; flatness by agreement. Narrow strip and cut plate to Annex A |
| Ultrasonic testing | Single-rolled plate 6 mm thick or thicker shall be tested to GB/T 2970-2016 Class II unless another method and class are agreed |
| Our supply | We produce and export Grade 20Cr to the GB/T 11251-2025 form, delivery condition, dimensions and extra tests agreed on the order |
Chemical composition of GB/T 11251 Grade 20Cr
GB/T 11251-2025 requires the grade and chemical composition to comply with GB/T 3077. The melt-analysis figures below are published GB/T 3077-2015 values for Grade 20Cr. They are not a separate chemistry table printed inside GB/T 11251-2025 itself, and they must not be read as an older GB/T 11251-2020 or GB/T 37601-2019 reprint labelled as 2025. Product-analysis tolerances shall meet GB/T 222; numeric product-analysis deviations are not listed here because a GB/T 222 table was not opened for this page.
| Element | Reference melt analysis (wt. %) |
|---|---|
| Carbon (C) | 0.18-0.24 |
| Silicon (Si) | 0.17-0.37 |
| Manganese (Mn) | 0.50-0.80 |
| Chromium (Cr) | 0.70-1.00 |
Phosphorus and sulfur depend on the GB/T 3077 quality class ordered: ordinary quality steel, high-quality steel designated by adding A, or extra-quality steel designated by adding E. Published secondary tables sometimes round those maxima; confirm the class and the limits on the mill test certificate. GB/T 11251-2025 also allows, by agreement on the contract, sulfur of 0.015% to 0.035% or not greater than 0.005%, or phosphorus not greater than 0.015%. Residual elements that are not specified alloying additions are limited by GB/T 3077.
Mechanical properties and optional tests
For annealed single-rolled plate of Grade 20Cr with nominal thickness not greater than 100 mm, GB/T 11251-2025 Table 1 specifies tensile strength Rm of 400-650 MPa and elongation A of not less than 20 %. For nominal thickness greater than 20 mm and not greater than 100 mm, elongation may be reduced by 0.25 % (absolute) for each 1 mm increase in thickness, but by not more than 5 % (absolute).
When single-rolled plate is delivered normalized, elongation shall still meet the Table 1 value and the upper limit of tensile strength may be 50 MPa higher than Table 1. High-temperature tempered single-rolled plate is ordered to surface hardness in accordance with GB/T 3077, not to the annealed Table 1 tensile band. Normalized-and-tempered and quenched-and-tempered single-rolled plate have mechanical properties agreed on the contract. Thickness greater than 100 mm is also by agreement.
Continuous-rolled plate and strip may be tensile-tested only by agreement; those results are not Table 1 values. Quenched-and-tempered GB/T 3077 bar figures must not be read as automatic GB/T 11251 plate minima.
Delivery conditions for GB/T 11251 Grade 20Cr
GB/T 11251-2025 distinguishes two product routes:
- Single-rolled plate is usually delivered high-temperature tempered. Annealed, normalized, normalized and tempered, or quenched and tempered supply may be agreed and written on the contract. Normalizing rolling may replace normalizing if the normalized mechanical requirements can be guaranteed.
- Continuous-rolled plate and strip are delivered as-rolled unless a heat-treatment condition is agreed. If they are spheroidize-annealed, surface hardness shall meet GB/T 3077.
We produce and export Grade 20Cr to the agreed route and condition. An enquiry that only says “20Cr plate” is incomplete, because high-temperature tempered, annealed, normalized and quenched-and-tempered plate are not interchangeable supply states, and single-rolled plate is not the same product as continuous-rolled plate or strip.
Welding and thermal cutting
Chromium 20Cr plate should be welded to a procedure suited to the grade, thickness and delivery condition. Preheat, interpass temperature and any post-weld heat treatment depend on thickness, joint restraint and the qualified procedure. Qualify cutting and welding procedures to the project specification, the ordered delivery condition and the actual thickness.
Thermal cutting can harden the adjacent material. That heat-affected zone should be considered, and removed where later forming or welding requires it.
Form, dimensions and inspection
Single-rolled plate dimensions, shape and mass tolerances follow GB/T 709-2019, with thickness tolerance class A unless another class is agreed. Wide strip and plate or slit strip cut from it follow GB/T 709-2019, using the thickness tolerances in Table 4 of that standard; flatness is agreed on the contract. Narrow strip and plate cut from it follow Annex A of GB/T 11251-2025. Other sizes and tolerances may be agreed.
Single-rolled plate 6 mm thick or thicker shall receive ultrasonic testing to GB/T 2970-2016 Class II unless another standard and class are written on the order. For stamping, single-rolled plate not thicker than 10 mm shall pass a 180° bend test with former diameter D = 2a.
Applications and specification limits
We produce and export this grade for general engineering parts that may later be carburized or otherwise heat treated after cutting. The carbon window sits above Grade 15Cr and well below through-hardening Grade 40Cr.
Do not confuse this grade with 20CrMo, which was not listed in the opened 2025 Table 1 and must not be claimed as the same plate grade.
GB/T 11251 is an alloy structural plate and strip specification. It is not a boiler or pressure-vessel book such as GB/T 713.
Compare GB/T 11251 20Cr with other steel plates
GB/T 11251 Grade 20Cr is alloy structural plate and strip under the 2025 Chinese plate book. The comparison below uses other plates we already publish. These grades are related by engineering use, not equivalents.
| Material | Alloy / type | Delivery condition | Mechanical requirements | Typical service | Substitution limit |
|---|---|---|---|---|---|
| GB/T 11251 Grade 20Cr (this plate) | Chromium alloy structural plate and strip under GB/T 11251-2025, higher carbon than Grade 15Cr and without a specified molybdenum range | Single-rolled: high-temperature tempered unless annealed, N, NT or QT is agreed. Continuous-rolled: as-rolled unless heat treated by agreement | Annealed single-rolled plate ≤ 100 mm: Rm 400-650 MPa and A ≥ 20 % (Table 1). Carburized-case properties are not Table 1 plate values | Engineering parts, often carburized or otherwise heat treated after cutting | Not 20CrMo, not Grade 15Cr or 40Cr, and not a 100 ksi QT structural grade |
| ASTM A829 4140 Alloy Steel Plate | Chromium-molybdenum alloy structural plate under ASTM A829/A829M, usually ordered by heat chemistry | AR, annealed, normalized, NT or QT as ordered | No automatic as-delivered strength package; tensile or hardness only if specified and compatible | Machinery and general engineering parts, often heat treated after cutting | Related alloy structural plate, not a GB/T 11251 equivalent and not a chromium-only or manganese grade substitute |
| ASTM A514 Grade B | Quenched-and-tempered alloy structural plate; chemistry includes chromium, molybdenum, vanadium, titanium and boron | Quenched and tempered | Strength-graded: to 32 mm, yield 100 ksi / 690 MPa min and tensile 110-130 ksi / 760-895 MPa (from our A514 Grade B page). Maximum thickness for Grade B is 1¼ in / 32 mm | Welded bridges and other structures that specify A514 QT plate | Not a substitute for chemistry-referenced GB/T 11251 engineering plate |
| ASTM A572 Grade 50 | High-strength low-alloy structural plate, microalloyed with niobium and vanadium | Hot-rolled or controlled-rolled | Strength-graded: minimum yield 345 MPa and tensile 450 MPa minimum (from our A572 Grade 50 page) | Bridges, buildings, construction equipment, transmission towers and heavy machinery frames | Not an alloy engineering plate of the GB/T 11251 type |
Related published ranges: Structural Steel Plates, ASTM A514/A514M and ASTM A572/A572M.
Equivalent and related grades by country
The designations below are near equivalents or related chemistry-family grades, not certified or automatic equivalents. Chemistry windows, product form, delivery condition and tests must match the project specification before a substitution is considered. Grades without a live page on this site are shown as plain text unless a live contrast page is named.
| Country / region | Standard | Grade | Similarity and key differences | Substitution caveat |
|---|---|---|---|---|
| China | GB/T 11251-2025 | 20Cr | This plate and strip specification. Table 1 lists annealed single-rolled tensile and elongation values for this grade at thickness not greater than 100 mm. | This product |
| China | GB/T 3077-2015 | 20Cr | The chemistry source cited by GB/T 11251-2025. GB/T 3077 is not a plate book. | Do not treat a 3077 bar enquiry as a 11251 plate order without restating product form, condition and tests. |
| China | GB/T 3077 / peer plate listings | 20CrMo | A molybdenum-bearing grade in the 3077 chemistry system. It was not listed in the opened GB/T 11251-2025 Table 1. | Not the same order code as 20Cr. Do not claim Table 1 listing without the 2025 table. |
| United States | AISI / SAE practice (via GB/T 3077 Annex A) | 5120 | Annex A of GB/T 3077-2015 lists 5120 as a similar designation. It is not an independent plate specification. | Not an automatic plate equivalent. |
| Europe | — | — | Case-hardening chromium grades are the usual European comparison family, not EN ISO 683-2 QT practice. A verified dedicated heat-analysis table was not opened for this page. | Do not assume a European case-hardening bar designation is a 11251 plate equivalent. |
| Japan | JIS G 4053 | SCr420 | Machine-structural chromium steel, not a plate book. Published SCr420 heat analysis: C 0.18-0.23, Si 0.15-0.35, Mn 0.60-0.90, P/S ≤ 0.030, Cr 0.90-1.20. Compared with published 3077 20Cr values (C 0.18-0.24, Mn 0.50-0.80, Cr 0.70-1.00), manganese and chromium windows differ. | Not an automatic plate equivalent. |
Grades 15Cr and 40Cr are related Table 1 chromium plate grades, not substitutes, and may not all have product pages on this site yet.
Why choose SHH STEEL for GB/T 11251 Grade 20Cr
- We produce and export GB/T 11251-2025 Grade 20Cr alloy structural steel plate
- We review the enquiry for edition, grade, product route, delivery condition, dimensions and extra tests
- We keep Table 1 annealed plate values distinct from high-temperature tempered hardness and from GB/T 3077 bar figures
- We match documentation to what the purchase order requires
How to enquire for GB/T 11251 20Cr plate
| Item | What to specify |
|---|---|
| Standard and grade | GB/T 11251-2025 Grade 20Cr |
| Product route | Single-rolled plate, or continuous-rolled plate or strip |
| Delivery condition | High-temperature tempered, annealed, normalized, normalized and tempered, quenched and tempered, or as-rolled for continuous-rolled material |
| Dimensions | Required thickness, width and length; we confirm production and export feasibility against the enquiry |
| Chemistry | Melt analysis to GB/T 3077, including any A or E quality class; request product analysis to GB/T 222 only if needed; state any agreed phosphorus or sulfur variant |
| Mechanical tests | State whether Table 1 annealed values, hardness, normalized values or an agreed quenched-and-tempered package applies |
| Other tests | Ultrasonic class if different from the standard Class II rule, bend testing for stamping, decarburization or inclusion rating only when written on the order |
| Documentation | State the inspection document type required by the project |
FAQ
-
Is GB/T 11251 20Cr ordered only by chemistry?
- Chemistry shall comply with GB/T 3077. For annealed single-rolled plate not thicker than 100 mm, Table 1 of GB/T 11251-2025 also sets tensile strength and elongation. High-temperature tempered plate is ordered to GB/T 3077 hardness. Other conditions are agreed on the contract.
-
Is GB/T 11251 20Cr the same as 20CrMo?
- No. 20CrMo adds molybdenum and was not listed in the opened 2025 Table 1. 20Cr is the chromium engineering grade with published Table 1 annealed plate values.
-
Does Table 1 apply to every delivery condition and thickness?
- No. Table 1 applies to annealed single-rolled plate not thicker than 100 mm. Normalized plate keeps the Table 1 elongation and may use a tensile upper limit 50 MPa higher. Thickness over 100 mm, continuous-rolled tensile tests, and NT or QT supply are by agreement.
-
Did GB/T 11251-2025 replace GB/T 37601?
- Yes. The 2025 edition replaces GB/T 11251-2020 and GB/T 37601-2019 and integrates the continuous-rolled content. Do not order this plate to the withdrawn 37601 book as if it were still current.
-
What should a quotation enquiry include?
- The ordered GB/T 11251 edition, Grade 20Cr, single-rolled or continuous-rolled route, delivery condition, thickness by width by length, quantity, any extra chemical or mechanical tests, any NDE, and the inspection document required by the project.
Request a quotation
Contact SHH STEEL for a quotation for GB/T 11251-2025 Grade 20Cr alloy steel plate. Please include your required quantity, plate thickness, width and length, whether you need single-rolled plate or continuous-rolled plate or strip, delivery destination and preferred delivery schedule so we can review your production and export requirements.
Specify the delivery condition. If your project requires tensile, hardness, toughness or ultrasonic testing beyond the standard rules, include the acceptance criteria and the inspection document required.
If you are considering 20CrMo, 15Cr, 40Cr or SCr420 as an alternative, send the applicable standard and project specification with your enquiry. We will review the differences in product form, chemistry and supply condition rather than assume that related grades are interchangeable.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.
Contact: admin@steelspecs.com