GB 712 Grade DH620 Shipbuilding Steel Plate

GB 712 Grade DH620 shipbuilding steel plate

GB 712 Grade DH620 extra-high-strength hull plate to the Chinese national standard GB 712 (IACS UR W16 basis): ReH 620 N/mm², Charpy −20 °C, TMCP or QT. Rolled to order at Chinese mills via SHH STEEL, with UT and 3.2 inspection.
Keywords
GB 712 DH620 steel plate, GB712 DH620 shipbuilding steel, GB 712 Grade DH620, DH620 extra high strength hull steel, Chinese standard offshore plate
Equivalent Grades:
CCS DH620; ABS DH62; DNV VL D620; LR DH62; BV D620; KR RD63; NK KD620; RINA D620; IACS UR W16 DH620
Share:
Overview
Specification
Chemical Composition
Mechanical Properties
Impact Test and Condition of Supply
Thickness Tolerance
Stock
Equivalent Grades
Grade Selection
Applications and Fabrication
Testing and Inspection
Specification Mistakes
Buyer Concerns
How to Order
FAQ
Conclusion

GB 712 Grade DH620 extra-high-strength shipbuilding steel plate — overview

Technical Reviewer: Jack | SHH STEEL Material Solutions Department · Updated: 2026-10-27

GB 712 Grade DH620 is the −20 °C grade at the 620 N/mm² extra-high-strength level of GB 712. GB 712 keeps the H in its extra-high-strength names and writes the yield in full — DH620 — in line with IACS UR W16 and with Chinese domestic usage. These grades let Chinese mills supply offshore and large-ship projects under the national standard (edition and table numbers not quoted — UNCERTAIN). The 620 level is a QT level for offshore and special structures, uncommon in conventional hulls.

Equivalent grades: ASTM A131 (no direct grade at this strength) · ABS DH62 / DQ63 · DNV NV D620 · LR DH62 · BV D620 · CCS DH620 · NK KD620 · KR RD63 · RINA D620.

Current edition: GB/T 712-2022 (Structural steel for ships and ocean engineering) (replaced GB 712-2011; implementation date 2023-05-01). English page titles keep the form “GB 712 Grade …”. Chemistry and tensile figures on this page are verified against the GB 712-2011 OCR tables and Caishuku consensus; full 2022 tables were not obtained free — do not assume 2022-only UHSS grades beyond this pack.

Requirements on the UR W16 basis: ReH ≥ 620 N/mm², Rm 720–890 N/mm², A ≥ 15 %, Charpy at −20 °C. The D letter is the one most often called for once EHS plate gets thick.

DH620 is produced TMCP or QT. In China it comes from the larger plate mills with heavy-plate lines, accelerated cooling and, at the upper levels, roller-quench and tempering furnaces (general context, not a claim about any single mill).

Unlike GB/T 1591 high-strength grades such as Q420 or Q460, GB 712 Grade DH620 carries hull-steel toughness grading, fine-grain practice and full alloy reporting, and it is the grade offshore and ship designers in China actually call for.

DH620 is rolled to order. SHH STEEL places it with a suitable Chinese mill, books any class survey or third-party witness, and adds UT and Z-direction testing on request. Typical uses: jack-up chords and racks, heavy-lift structure and special offshore steelwork, as QT plate.

How GB 712 names it. DH620 = toughness letter D, H for higher strength, and the full minimum yield 620 N/mm². At 620 only a limited group of Chinese mills produce the grade; plan early.

GB 712 Grade DH620: key data at a glance

ItemGB 712 Grade DH620
StandardGB 712, extra-high-strength hull and offshore structural steel; IACS UR W16 basis (GB 712 clause/table numbers not quoted — UNCERTAIN)
DesignationDH620: toughness letter D + H + minimum yield 620 N/mm²
StrengthReH ≥ 620, Rm 720–890 N/mm², A ≥ 15 %
Charpy V−20 °C; average ≥ 62 J L / 41 J T (UR W16-aligned — confirm)
Condition of supplyTMCP or QT within the mill’s qualified thickness range
Steelmakingkilled, fine-grain; vacuum degassing and Ca treatment typical
UTnormally specified — GB/T 2970 or agreed export standard
DimensionsGB/T 709 or agreed export standard
Certificatebilingual GB 712 certificate with Ceq / CET / Pcm; class or EN 10204 3.2 on request

Maximum thickness depends on the mill and route. As a guide, TMCP DH620 is often offered to about 50–80 mm and QT thicker (UNCERTAIN). At this level most enquiries are 20–100 mm QT plate for offshore and lifting structure.

GB 712 Grade DH620 chemistry — full alloy list including B

ElementHeat (ladle) analysis, %Product (check) analysis, %Comment
C0.21 max. (often 0.14–0.20 by route/condition; TM/QT may tighten)0.23 max. (0.21 + 0.02)
Si0.55 max. (QT may allow up to ~0.80 — confirm on mill approval)0.60 max. (0.55 + 0.05)
Mn1.70 max. (typically 1.00–1.70; QT route may differ)1.76 max. (1.70 + 0.06)
P0.025 max. (some EQ-style routes tighter — confirm)0.030 max. (0.025 + 0.005)
S0.025 max. (some EQ-style routes tighter — confirm)0.030 max. (0.025 + 0.005)
Al0.015 min. acid-soluble / ≈0.020 total Al (fine-grain; Al/N control unless other N-binders)0.012 min. (0.015 − 0.003)grain refiner / N binder
Nb0.05 max. (when used; combined microalloy caps apply)0.055 max. (0.05 + 0.005)
V0.10 max. (when used; combined caps apply)0.12 max. (0.10 + 0.02)
Ti0.05 max. (when used; combined caps apply)0.07 max. (0.05 + 0.02)
Cu0.50 max. (route-dependent; often ≤0.35 in practice)0.55 max. (0.50 + 0.05)
Cr0.20–0.25 max. (route-dependent)0.25–0.30 max. (each heat max.: 0.20 + 0.05; 0.25 + 0.05)
Ni2.00 max. or per mill approval (often lower on AH/DH routes)2.00 max. (value outside the GB/T 222-2006 Table 1 Ni rows – no tabulated deviation; agree on order)toughness
Mo0.08–0.50 (route-dependent; QT may allow higher)0.08–0.50 (Mo not listed in GB/T 222-2006 Table 1 – heat limit applies)hardenability (QT)
B0.005 max. (when intentionally added)0.005 max. (B not listed in GB/T 222-2006 Table 1 – heat limit applies)hardenability (QT)
N0.015 max. (tighter control when Al is the sole N-binder)0.020 max. (0.015 + 0.005)
Nb+V+TiNb+V+Ti typically < 0.26 % for N/TM routes (not QT) — confirm UR W16 / mill approvalnot applicable (calculated from heat analysis)combined
Ceq / CET / PcmCeq / CET / Pcm maxima by category and condition on mill approval — report on certificatenot applicable (calculated from heat analysis)calculated

Product (check) analysis column = heat (ladle) limit adjusted by GB/T 222-2006 Table 1 (non-alloy and low-alloy steel), as invoked by GB 712 clause 6.1.3 (upper limit + upper deviation, lower limit − lower deviation; row chosen by the specified upper limit; values for cross-sections up to 6 500 mm², larger sections by agreement); arithmetic shown in brackets.

The table gives the UR W16 envelope that GB 712 follows for extra-high-strength steel; individual mills hold tighter internal limits, and the GB 712 text governs (not checked locally — UNCERTAIN). At 620, a boron-bearing Ni–Cr–Mo QT steel is typical; welders watch Pcm closely.

The D letter shares the A/D/E envelope; toughness comes mainly from process route and cleanliness. Every intentionally added element must appear on the certificate together with Ceq, CET or Pcm.

Boron, when added, works in parts per million and only when nitrogen is tied up, usually by titanium; read B, Ti and N together on the certificate.

For EHS plate the certificate should also state the formula used for Ceq, CET and Pcm, since different mills and owners use different ones.

GB 712 Grade DH620 tensile and impact requirements

PropertyRequirement
ReH (or Rp0.2)620 N/mm² min.
Rm720–890 N/mm²
A15 % min.
Charpy V−20 °C, ≥ 62 J L / 41 J T (average)
Yield/tensile ratioreport; limit only if ordered

Tests are taken per heat-treatment batch or rolled length; thick plate may need mid-thickness tests. Against DH40 the yield rises by 230 N/mm². The gain only counts if the welded joint keeps up, so qualify the procedure for matching strength and toughness in weld metal and HAZ.

Tensile specimens are taken transverse to the rolling direction for plate, following UR W11/W16 practice; the certificate should show the specimen orientation and type. For QT plate Rp0.2 is often reported, because the yield point is not pronounced.

GB 712 Grade DH620: toughness at −20 °C and TMCP vs QT

Charpy specimens are usually taken at quarter thickness and tested at −20 °C. Delivery is TMCP or QT, and the route changes mill choice, price, flatness and welding behaviour, so state it on the order. QT is the usual route at this level, especially in thick plate.

Strain-ageing or CTOD data are not part of the basic grade; ask only if your specification requires them.

TMCP plate gets its strength from controlled rolling and accelerated cooling, so it starts with low carbon and good weldability but can lose strength if overheated. QT plate is austenitised, quenched and tempered, giving uniform properties through thick sections; the tempering temperature then caps any later heat treatment.

Thickness tolerance and flatness

Plates are rolled to GB/T 709 or an agreed export standard with a hull-steel minus tolerance (UR W13 practice — confirm). QT plate is generally flatter but harder to straighten later, so agree the flatness class at enquiry. Do not flame-straighten EHS plate above the mill’s stated temperature; it can undo the TMCP or tempering treatment.

If the plate is ordered with a classification certificate, the class minus tolerance applies whatever dimension standard is named, so state both on the order. For EHS plate, ask for ultrasonic thickness readings to be recorded if the design relies on the minimum thickness.

GB 712 Grade DH620 mill-rolled supply

Thickness (mm)Width (mm)ConditionTypical lot
122000 / 2500TMCP / QTper heat / rolling
162200 / 2500TMCP / QTper heat / rolling
202500TMCP / QTper heat / rolling
252500TMCP / QTper heat / rolling
302200 / 2500TMCP / QTper heat / rolling
402200TMCP / QTper heat / rolling
502200TMCP / QTper heat / rolling

GB 712 Grade DH620 is not held as open stock. The table shows the sizes most often booked into a mill campaign; expect roughly 6–10 weeks from order to certified plate (commercial estimate).

Packing and shipping: bundled by size with steel strapping, stencilled with standard, grade and heat number, and shipped from Shanghai, Tianjin, Qingdao or other Chinese ports in containers (≤ 11.8 m) or break bulk.

Processing before shipping. We cut DH620 to drawing by plasma or oxy-fuel, bevel edges, shot-blast and prime, and transfer grade, heat and plate number to every piece so that GB 712 traceability survives cutting. Cut parts ship with a cutting list cross-referencing each piece to its mother plate and certificate.

GB 712 Grade DH620 against class societies

Standard / societyDesignationRemark
GB 712 (this page)GB 712 Grade DH620Chinese national product standard; no class stamp by itself
CCSCCS DH620same letters as GB 712; the usual class mark on domestic Chinese hulls
ABSABS DH62EHS numbered by yield/10
DNVDNV VL D620VL prefix
LRLR DH62EHS numbered by yield/10
BVBV D620EHS written without H
KRKR RD63R-prefix
NKNK KD620K-prefix
RINARINA D620EHS written without H
ASTM A131noneA131 stops at FH40

GB 712 and the CCS Rules. GB 712 was drafted to mirror the IACS unified requirements, which the China Classification Society (CCS) also applies in its Rules for Materials and Welding. In practice a Chinese mill rolls one heat to the shared chemistry and test plan; the plate becomes GB 712 Grade DH620 through the national standard and CCS DH620 through CCS survey. The two are parallel documents, not one replacing the other (CCS chapter numbering not quoted — UNCERTAIN).

Class certification on a GB 712 base. Export buyers often order “GB 712 DH620 with CCS, ABS or DNV certificate” (or another IACS society). The class surveyor must witness or audit the tests at the mill before shipment; a plain GB 712 certificate cannot be converted into a class certificate afterwards. Several marks on one plate are possible when every society is booked in advance and the mill holds the relevant approvals.

Where DH620 sits in the GB 712 AH420–FH690 series

Neighbours are DH550 below and DH690 above. Within level 620 the letter sets the test temperature: A 0 °C, D −20 °C, E −40 °C, F −60 °C.

For a yield-governed member, 30 mm of DH40 becomes roughly 18.9 mm of DH620; buckling, fatigue and corrosion margins usually make the real saving smaller (estimate, not a rule value).

Other GB 712 grades are under GB 712 shipbuilding steel plates; offshore-specific grades under offshore platform steel plates.

EHS grades are usually concentrated in a few highly stressed areas rather than used everywhere. That keeps the number of welding procedures down: the yard only needs DH620 procedures where it pays. DH is often the best-value letter where the drawing allows a choice between AH and EH.

Fabricating GB 712 Grade DH620

Typical uses: jack-up chords and racks, heavy-lift structure and special offshore steelwork, as QT plate.

Weld DH620 only under a qualified WPS for this grade, with low-hydrogen consumables reaching matching strength and −20 °C toughness in the weld metal. Limit heat input to protect HAZ toughness in QT plate; thick sections usually need preheat. Do not hot-form or stress-relieve above the tempering temperature without the mill’s agreement.

HAZ softening can occur in TMCP plate under very high heat input and HAZ hardening in QT plate under very low heat input, so respect both ends of the qualified range. Hydrogen control — dry consumables, clean joints, controlled preheat — matters more as strength rises.

GB 712 tests, certificate and receiving checks

The certificate gives full alloy analysis, Ceq/CET/Pcm, tensile results, −20 °C Charpy results, condition of supply, UT result and plate numbers, in Chinese and English.

On receipt, check the DH620 stencil, impact temperature, UT report and heat numbers. Third-party witness and class survey must be booked before rolling.

Mill quality system. Chinese plate mills supplying GB 712 normally run ISO 9001-certified quality systems and hold their own national product certification; when a class certificate is wanted, the mill must also hold that society’s works approval for the grade and thickness (details per mill — UNCERTAIN). Ask for that approval scope before ordering; it is the single most useful check a buyer can make.

Mistakes we see on GB 712 Grade DH620 orders

  • Ordering GB/T 1591 Q620 instead of DH620
  • Leaving TMCP vs QT open
  • No UT requirement
  • Ceq/Pcm not requested
  • Choosing a mill without proven production of this grade and thickness
  • Expecting an ASTM A131 equivalent (none exists at this level)

EHS plate is rolled for you, so a wrong order line costs a full rolling cycle. Check it twice.

With EHS plate the costly errors cannot be fixed after rolling: wrong route, a thickness outside what the mill has produced, or missing UT.

Buying GB 712 Grade DH620 from China: concerns and answers

ConcernAnswer
Is the certificate genuine?Original mill certificate for GB 712 Grade DH620, traceable by heat and plate number; mill verification and third-party witness on request
Will a foreign yard or inspector read it?Bilingual Chinese/English certificate; supply-condition codes translated
Export paperworkcommercial invoice, packing list, bill of lading, certificate of origin (Form E or general CO on request)
Payment safetyT/T with balance after inspection, or L/C at sight
Small or mixed orderssizes grouped onto one heat where possible
Ready-to-fit partscutting, bevelling, shot-blasting and priming in our own workshop

If you have not bought GB 712 plate from China before, we can send sample certificates in advance, arrange a trial lot, and let your inspector visit the mill during rolling and testing. For buyers outside China we also check that the bilingual certificate wording matches the purchase order line by line before shipment.

Ordering GB 712 Grade DH620

State GB 712 DH620, TMCP or QT, sizes and quantities, UT level, any class certificate, certificate type and port, and send to SHH STEEL.

Sample line: “Plate to GB 712, grade DH620, QT, 40 × 2500 × 10000 mm, 8 pcs, UT to GB/T 2970, bilingual certificate with Pcm, EN 10204 3.2.”

Order checklist:

  • Standard: GB 712 (state edition if your contract requires one)
  • Grade: DH620
  • Condition of supply (TMCP or QT)
  • Sizes and quantity per size; tolerance standard and flatness class
  • Certificate: bilingual GB 712 mill certificate, EN 10204 3.1 or 3.2; class certificate if required
  • Extras: UT, Z-direction, shot-blast/prime, cutting
  • Delivery terms, destination port and documents (CO, Form E)

FAQ

Why does GB 712 write DH620 with an H?
GB 712 keeps the H for all higher-strength hull steels and writes the extra-high levels with the full yield, so DH620 = letter D, yield 620 N/mm². Some other naming systems drop the H or divide the number by ten; it is the same UR W16 level. On RFQs from China you may also see “DH620” written in Chinese documents as DH620; it is the same grade, and the stencil should read DH620. In short, DH620 under GB 712 is defined by its letter and strength level; the Chinese standard, the IACS unified requirement and the classification rules all describe the same steel from different angles, so a clear order line covering standard, grade and certificate type removes most confusion. DH is commonly rolled from the same heats as EH. Because DH620 is outside the range of ASTM A131, US-based buyers usually reference GB 712 or a class grade directly.
What does DH620 guarantee?
ReH ≥ 620 N/mm², Rm 720–890 N/mm², A ≥ 15 % and a Charpy average of at least 62 J longitudinal or 41 J transverse at −20 °C (UR W16-aligned; confirm on the certificate). At 620 N/mm² yield the tensile window 720–890 N/mm² is wide; ask the mill for typical results on your thickness to judge consistency. At 620 only a limited group of Chinese mills produce the grade; plan early. When comparing certificates from different Chinese mills, compare the average and the lowest single Charpy value at −20 °C, not only whether the plate passed; a comfortable margin is the better sign of a stable process. At 620 hydrogen control in welding becomes a decisive quality factor. Charpy energy for DH620 is set higher than for level-40 plate, reflecting the higher strength.
TMCP or QT for DH620?
QT is the usual route at this level, especially in thick plate. The route changes price, flatness and the welding procedure, so state it on the order. For DH620, TMCP is uncommon at this strength, and QT gives more uniform through-thickness properties in heavy plate. For design offices outside China, GB 712 is a convenient reference because it uses the same letters and levels as the IACS tables; the drawing can say DH620 and the class requirement in one line, and the mill will understand both. TMCP and QT certificates look similar, so check the delivery-condition line before anything else, then the heat-treatment temperatures if the plate is QT.
Is DH620 available from stock?
Rarely. DH620 is rolled to order, typically in 6–10 weeks including testing. Order planning matters: the rolling slot is booked first, then testing and any survey, then shipping, so confirm drawings early. Typical DH620 enquiries from export buyers come with a cutting list and a delivery schedule by block; sending both early lets the mill group sizes and saves rolling slots. Large orders can be split into several heats; each heat then carries its own full test set, and grouping sizes by heat keeps the number of tests, and the cost of survey, under control.
Which elements appear on the certificate?
C, Si, Mn, P, S, Al, Nb, V, Ti, Cu, Cr, Ni, Mo, B and N, plus Nb+V+Ti and Ceq, CET or Pcm. Pcm is especially relevant for low-carbon QT chemistries, where Ceq can understate hardening tendency; the WPS should state which index it uses. Any change of grade after the mill has rolled the plate means new plate; there is no way to re-grade DH620 on paper once the tests are done. Boron-bearing grades need B reported to three decimals or in ppm so the welding engineer can assess it.
Where is DH620 used?
Typical uses: jack-up chords and racks, heavy-lift structure and special offshore steelwork, as QT plate. The D letter suits members designed for −20 °C toughness. On offshore units EHS plate is usually concentrated in legs, chords, racks, crane pedestals and highly stressed nodes; the hull plating is typically still AH/DH36. If a class certificate is needed, booking the surveyor before rolling is the step that decides whether DH620 can be delivered on time; we arrange it with the mill when the order is placed. Designers should confirm weld-metal toughness at the same temperature as the plate.
Is DH620 the same as GB/T 1591 Q620?
No. Q-grades are general structural steels; DH620 is hull and offshore steel with letter-graded toughness at −20 °C and full alloy reporting. Q620 plate to GB/T 1591 may be offered at a lower price; it does not carry the hull-steel toughness grading and is not a substitute. Keep preheat and interpass temperatures for DH620 within the WPS range. For DH620, ask the mill to state plate weight on the certificate as theoretical or actual weight, because Chinese invoices may use either and the difference matters on large orders. A GB/T 1591 Q-grade certificate shows no letter-graded Charpy line, which makes the difference easy to spot.
What are payment terms and inspection options?
T/T deposit with balance after inspection, or L/C at sight. UT, EN 10204 3.2 witness and class survey can be added if booked before rolling. Mill inspection can be combined with UT witnessing to save one visit; book both before rolling, and allow for export documents such as the certificate of origin. Quotations for DH620 are normally valid for a short period because Chinese plate prices move with iron ore and coking coal; fix price and rolling slot together. Third-party inspectors familiar with Chinese heavy-plate mills can shorten the witness programme.

Conclusion

GB 712 Grade DH620 is the extra-high-strength hull structural steel of the Chinese national standard GB 712, on the IACS UR W16 basis: yield 620 N/mm², tensile 720–890 N/mm², Charpy −20 °C. Order it by standard and grade, and add a classification certificate on the same heat when the hull is classed.

SHH STEEL supplies GB 712 Grade DH620 from Chinese mills with bilingual certificates, cutting, UT and EN 10204 3.2 on request. Send grade, sizes, quantities and port for a quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *



    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *



      X