GB 712 Grade DH550 shipbuilding steel plate
GB 712 Grade DH550 extra-high-strength shipbuilding steel plate — overview
GB 712 Grade DH550 is the −20 °C grade at the 550 N/mm² extra-high-strength level of GB 712. GB 712 keeps the H in its extra-high-strength names and writes the yield in full — DH550 — in line with IACS UR W16 and with Chinese domestic usage. These grades let Chinese mills supply offshore and large-ship projects under the national standard (edition and table numbers not quoted — UNCERTAIN). The 550 level is normally quenched and tempered, used for jack-up legs, crane booms and heavily loaded offshore members.
Equivalent grades: ASTM A131 (no direct grade at this strength) · ABS DH55 / DQ56 · DNV NV D550 · LR DH55 · BV D550 · CCS DH550 · NK KD550 · KR RD56 · RINA D550.
Current edition: GB/T 712-2022 (Structural steel for ships and ocean engineering) (replaced GB 712-2011; implementation date 2023-05-01). English page titles keep the form “GB 712 Grade …”. Chemistry and tensile figures on this page are verified against the GB 712-2011 OCR tables and Caishuku consensus; full 2022 tables were not obtained free — do not assume 2022-only UHSS grades beyond this pack.
Requirements on the UR W16 basis: ReH ≥ 550 N/mm², Rm 670–835 N/mm², A ≥ 16 %, Charpy at −20 °C. The D letter is the one most often called for once EHS plate gets thick.
DH550 is produced TMCP or QT. In China it comes from the larger plate mills with heavy-plate lines, accelerated cooling and, at the upper levels, roller-quench and tempering furnaces (general context, not a claim about any single mill).
Unlike GB/T 1591 high-strength grades such as Q420 or Q460, GB 712 Grade DH550 carries hull-steel toughness grading, fine-grain practice and full alloy reporting, and it is the grade offshore and ship designers in China actually call for.
DH550 is rolled to order. SHH STEEL places it with a suitable Chinese mill, books any class survey or third-party witness, and adds UT and Z-direction testing on request. Typical uses: jack-up legs, crane booms and highly loaded offshore members, mostly quenched and tempered plate.
How GB 712 names it. DH550 = toughness letter D, H for higher strength, and the full minimum yield 550 N/mm². At 550 QT is the norm and lead times lengthen.
GB 712 Grade DH550: key data at a glance
| Item | GB 712 Grade DH550 |
|---|---|
| Standard | GB 712, extra-high-strength hull and offshore structural steel; IACS UR W16 basis (GB 712 clause/table numbers not quoted — UNCERTAIN) |
| Designation | DH550: toughness letter D + H + minimum yield 550 N/mm² |
| Strength | ReH ≥ 550, Rm 670–835 N/mm², A ≥ 16 % |
| Charpy V | −20 °C; average ≥ 55 J L / 37 J T (UR W16-aligned — confirm) |
| Condition of supply | TMCP or QT within the mill’s qualified thickness range |
| Steelmaking | killed, fine-grain; vacuum degassing and Ca treatment typical |
| UT | normally specified — GB/T 2970 or agreed export standard |
| Dimensions | GB/T 709 or agreed export standard |
| Certificate | bilingual GB 712 certificate with Ceq / CET / Pcm; class or EN 10204 3.2 on request |
Maximum thickness depends on the mill and route. As a guide, TMCP DH550 is often offered to about 50–80 mm and QT thicker (UNCERTAIN). At this level most enquiries are 20–100 mm QT plate for offshore and lifting structure.
GB 712 Grade DH550 chemistry — full alloy list including B
| Element | Heat (ladle) analysis, % | Product (check) analysis, % | Comment |
|---|---|---|---|
| C | 0.21 max. (often 0.14–0.20 by route/condition; TM/QT may tighten) | 0.23 max. (0.21 + 0.02) | |
| Si | 0.55 max. (QT may allow up to ~0.80 — confirm on mill approval) | 0.60 max. (0.55 + 0.05) | |
| Mn | 1.70 max. (typically 1.00–1.70; QT route may differ) | 1.76 max. (1.70 + 0.06) | |
| P | 0.025 max. (some EQ-style routes tighter — confirm) | 0.030 max. (0.025 + 0.005) | |
| S | 0.025 max. (some EQ-style routes tighter — confirm) | 0.030 max. (0.025 + 0.005) | |
| Al | 0.015 min. acid-soluble / ≈0.020 total Al (fine-grain; Al/N control unless other N-binders) | 0.012 min. (0.015 − 0.003) | grain refiner / N binder |
| Nb | 0.05 max. (when used; combined microalloy caps apply) | 0.055 max. (0.05 + 0.005) | |
| V | 0.10 max. (when used; combined caps apply) | 0.12 max. (0.10 + 0.02) | |
| Ti | 0.05 max. (when used; combined caps apply) | 0.07 max. (0.05 + 0.02) | |
| Cu | 0.50 max. (route-dependent; often ≤0.35 in practice) | 0.55 max. (0.50 + 0.05) | |
| Cr | 0.20–0.25 max. (route-dependent) | 0.25–0.30 max. (each heat max.: 0.20 + 0.05; 0.25 + 0.05) | |
| Ni | 2.00 max. or per mill approval (often lower on AH/DH routes) | 2.00 max. (value outside the GB/T 222-2006 Table 1 Ni rows – no tabulated deviation; agree on order) | toughness |
| Mo | 0.08–0.50 (route-dependent; QT may allow higher) | 0.08–0.50 (Mo not listed in GB/T 222-2006 Table 1 – heat limit applies) | hardenability (QT) |
| B | 0.005 max. (when intentionally added) | 0.005 max. (B not listed in GB/T 222-2006 Table 1 – heat limit applies) | hardenability (QT) |
| N | 0.015 max. (tighter control when Al is the sole N-binder) | 0.020 max. (0.015 + 0.005) | |
| Nb+V+Ti | Nb+V+Ti typically < 0.26 % for N/TM routes (not QT) — confirm UR W16 / mill approval | not applicable (calculated from heat analysis) | combined |
| Ceq / CET / Pcm | Ceq / CET / Pcm maxima by category and condition on mill approval — report on certificate | not applicable (calculated from heat analysis) | calculated |
Product (check) analysis column = heat (ladle) limit adjusted by GB/T 222-2006 Table 1 (non-alloy and low-alloy steel), as invoked by GB 712 clause 6.1.3 (upper limit + upper deviation, lower limit − lower deviation; row chosen by the specified upper limit; values for cross-sections up to 6 500 mm², larger sections by agreement); arithmetic shown in brackets.
The table gives the UR W16 envelope that GB 712 follows for extra-high-strength steel; individual mills hold tighter internal limits, and the GB 712 text governs (not checked locally — UNCERTAIN). At 550, a quenched and tempered Ni–Cr–Mo steel, sometimes boron-treated, is usual.
The D letter shares the A/D/E envelope; toughness comes mainly from process route and cleanliness. Every intentionally added element must appear on the certificate together with Ceq, CET or Pcm.
Boron, when added, works in parts per million and only when nitrogen is tied up, usually by titanium; read B, Ti and N together on the certificate.
For EHS plate the certificate should also state the formula used for Ceq, CET and Pcm, since different mills and owners use different ones.
GB 712 Grade DH550 tensile and impact requirements
| Property | Requirement |
|---|---|
| ReH (or Rp0.2) | 550 N/mm² min. |
| Rm | 670–835 N/mm² |
| A | 16 % min. |
| Charpy V | −20 °C, ≥ 55 J L / 37 J T (average) |
| Yield/tensile ratio | report; limit only if ordered |
Tests are taken per heat-treatment batch or rolled length; thick plate may need mid-thickness tests. Against DH40 the yield rises by 160 N/mm². The gain only counts if the welded joint keeps up, so qualify the procedure for matching strength and toughness in weld metal and HAZ.
Tensile specimens are taken transverse to the rolling direction for plate, following UR W11/W16 practice; the certificate should show the specimen orientation and type. For QT plate Rp0.2 is often reported, because the yield point is not pronounced.
GB 712 Grade DH550: toughness at −20 °C and TMCP vs QT
Charpy specimens are usually taken at quarter thickness and tested at −20 °C. Delivery is TMCP or QT, and the route changes mill choice, price, flatness and welding behaviour, so state it on the order. QT is the usual route at this level, especially in thick plate.
Strain-ageing or CTOD data are not part of the basic grade; ask only if your specification requires them.
TMCP plate gets its strength from controlled rolling and accelerated cooling, so it starts with low carbon and good weldability but can lose strength if overheated. QT plate is austenitised, quenched and tempered, giving uniform properties through thick sections; the tempering temperature then caps any later heat treatment.
Thickness tolerance and flatness
Plates are rolled to GB/T 709 or an agreed export standard with a hull-steel minus tolerance (UR W13 practice — confirm). QT plate is generally flatter but harder to straighten later, so agree the flatness class at enquiry. Do not flame-straighten EHS plate above the mill’s stated temperature; it can undo the TMCP or tempering treatment.
If the plate is ordered with a classification certificate, the class minus tolerance applies whatever dimension standard is named, so state both on the order. For EHS plate, ask for ultrasonic thickness readings to be recorded if the design relies on the minimum thickness.
GB 712 Grade DH550 mill-rolled supply
| Thickness (mm) | Width (mm) | Condition | Typical lot |
|---|---|---|---|
| 12 | 2000 / 2500 | TMCP / QT | per heat / rolling |
| 16 | 2200 / 2500 | TMCP / QT | per heat / rolling |
| 20 | 2500 | TMCP / QT | per heat / rolling |
| 25 | 2500 | TMCP / QT | per heat / rolling |
| 30 | 2200 / 2500 | TMCP / QT | per heat / rolling |
| 40 | 2200 | TMCP / QT | per heat / rolling |
| 50 | 2200 | TMCP / QT | per heat / rolling |
GB 712 Grade DH550 is not held as open stock. The table shows the sizes most often booked into a mill campaign; expect roughly 6–10 weeks from order to certified plate (commercial estimate).
Packing and shipping: bundled by size with steel strapping, stencilled with standard, grade and heat number, and shipped from Shanghai, Tianjin, Qingdao or other Chinese ports in containers (≤ 11.8 m) or break bulk.
Processing before shipping. We cut DH550 to drawing by plasma or oxy-fuel, bevel edges, shot-blast and prime, and transfer grade, heat and plate number to every piece so that GB 712 traceability survives cutting. Cut parts ship with a cutting list cross-referencing each piece to its mother plate and certificate.
GB 712 Grade DH550 against class societies
| Standard / society | Designation | Remark |
|---|---|---|
| GB 712 (this page) | GB 712 Grade DH550 | Chinese national product standard; no class stamp by itself |
| CCS | CCS DH550 | same letters as GB 712; the usual class mark on domestic Chinese hulls |
| ABS | ABS DH55 | EHS numbered by yield/10 |
| DNV | DNV VL D550 | VL prefix |
| LR | LR DH55 | EHS numbered by yield/10 |
| BV | BV D550 | EHS written without H |
| KR | KR RD56 | R-prefix |
| NK | NK KD550 | K-prefix |
| RINA | RINA D550 | EHS written without H |
| ASTM A131 | none | A131 stops at FH40 |
GB 712 and the CCS Rules. GB 712 was drafted to mirror the IACS unified requirements, which the China Classification Society (CCS) also applies in its Rules for Materials and Welding. In practice a Chinese mill rolls one heat to the shared chemistry and test plan; the plate becomes GB 712 Grade DH550 through the national standard and CCS DH550 through CCS survey. The two are parallel documents, not one replacing the other (CCS chapter numbering not quoted — UNCERTAIN).
Class certification on a GB 712 base. Export buyers often order “GB 712 DH550 with CCS, ABS or DNV certificate” (or another IACS society). The class surveyor must witness or audit the tests at the mill before shipment; a plain GB 712 certificate cannot be converted into a class certificate afterwards. Several marks on one plate are possible when every society is booked in advance and the mill holds the relevant approvals.
Where DH550 sits in the GB 712 AH420–FH690 series
Neighbours are DH500 below and DH620 above. Within level 550 the letter sets the test temperature: A 0 °C, D −20 °C, E −40 °C, F −60 °C.
For a yield-governed member, 30 mm of DH40 becomes roughly 21.3 mm of DH550; buckling, fatigue and corrosion margins usually make the real saving smaller (estimate, not a rule value).
Other GB 712 grades are under GB 712 shipbuilding steel plates; offshore-specific grades under offshore platform steel plates.
EHS grades are usually concentrated in a few highly stressed areas rather than used everywhere. That keeps the number of welding procedures down: the yard only needs DH550 procedures where it pays. DH is often the best-value letter where the drawing allows a choice between AH and EH.
Fabricating GB 712 Grade DH550
Typical uses: jack-up legs, crane booms and highly loaded offshore members, mostly quenched and tempered plate.
Weld DH550 only under a qualified WPS for this grade, with low-hydrogen consumables reaching matching strength and −20 °C toughness in the weld metal. Limit heat input to protect HAZ toughness in QT plate; thick sections usually need preheat. Do not hot-form or stress-relieve above the tempering temperature without the mill’s agreement.
HAZ softening can occur in TMCP plate under very high heat input and HAZ hardening in QT plate under very low heat input, so respect both ends of the qualified range. Hydrogen control — dry consumables, clean joints, controlled preheat — matters more as strength rises.
GB 712 tests, certificate and receiving checks
The certificate gives full alloy analysis, Ceq/CET/Pcm, tensile results, −20 °C Charpy results, condition of supply, UT result and plate numbers, in Chinese and English.
On receipt, check the DH550 stencil, impact temperature, UT report and heat numbers. Third-party witness and class survey must be booked before rolling.
Mill quality system. Chinese plate mills supplying GB 712 normally run ISO 9001-certified quality systems and hold their own national product certification; when a class certificate is wanted, the mill must also hold that society’s works approval for the grade and thickness (details per mill — UNCERTAIN). Ask for that approval scope before ordering; it is the single most useful check a buyer can make.
Mistakes we see on GB 712 Grade DH550 orders
- Ordering GB/T 1591 Q550 instead of DH550
- Leaving TMCP vs QT open
- No UT requirement
- Ceq/Pcm not requested
- Choosing a mill without proven production of this grade and thickness
- Expecting an ASTM A131 equivalent (none exists at this level)
EHS plate is rolled for you, so a wrong order line costs a full rolling cycle. Check it twice.
With EHS plate the costly errors cannot be fixed after rolling: wrong route, a thickness outside what the mill has produced, or missing UT.
Buying GB 712 Grade DH550 from China: concerns and answers
| Concern | Answer |
|---|---|
| Is the certificate genuine? | Original mill certificate for GB 712 Grade DH550, traceable by heat and plate number; mill verification and third-party witness on request |
| Will a foreign yard or inspector read it? | Bilingual Chinese/English certificate; supply-condition codes translated |
| Export paperwork | commercial invoice, packing list, bill of lading, certificate of origin (Form E or general CO on request) |
| Payment safety | T/T with balance after inspection, or L/C at sight |
| Small or mixed orders | sizes grouped onto one heat where possible |
| Ready-to-fit parts | cutting, bevelling, shot-blasting and priming in our own workshop |
If you have not bought GB 712 plate from China before, we can send sample certificates in advance, arrange a trial lot, and let your inspector visit the mill during rolling and testing. For buyers outside China we also check that the bilingual certificate wording matches the purchase order line by line before shipment.
Ordering GB 712 Grade DH550
State GB 712 DH550, TMCP or QT, sizes and quantities, UT level, any class certificate, certificate type and port, and send to SHH STEEL.
Sample line: “Plate to GB 712, grade DH550, QT, 40 × 2500 × 10000 mm, 8 pcs, UT to GB/T 2970, bilingual certificate with Pcm, EN 10204 3.2.”
Order checklist:
- Standard: GB 712 (state edition if your contract requires one)
- Grade: DH550
- Condition of supply (TMCP or QT)
- Sizes and quantity per size; tolerance standard and flatness class
- Certificate: bilingual GB 712 mill certificate, EN 10204 3.1 or 3.2; class certificate if required
- Extras: UT, Z-direction, shot-blast/prime, cutting
- Delivery terms, destination port and documents (CO, Form E)
FAQ
Conclusion
GB 712 Grade DH550 is the extra-high-strength hull structural steel of the Chinese national standard GB 712, on the IACS UR W16 basis: yield 550 N/mm², tensile 670–835 N/mm², Charpy −20 °C. Order it by standard and grade, and add a classification certificate on the same heat when the hull is classed.
SHH STEEL supplies GB 712 Grade DH550 from Chinese mills with bilingual certificates, cutting, UT and EN 10204 3.2 on request. Send grade, sizes, quantities and port for a quotation.