BS 1501 224 Grade 490B Steel Plate
What is BS 1501-224 Grade 490B plate?
We produce and export BS 1501-224 Grade 490B as fully killed aluminium-treated carbon-manganese steel plate for fired and unfired pressure equipment. Typical service includes welded boilers and vessels that specify type 224 grade 490B.
BS 1501-1:1980 lists eight steel types, each with one or more tensile grades and, where Table 1 allows, suffix A or B and optional impact suffixes. This page specifies only 224 Grade 490B. It is not type 223 or 225, grade 460 of the same type, or a BS 1501-2 alloy plate. Suffix B specifies room-temperature tensile properties together with characteristic elevated-temperature values.
Composition and room-temperature tensile properties on this page follow BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates, the last final edition of Part 1. BS 1501-1:1980 was published on 28 November 1980 and withdrawn on 15 February 1993. It replaced BS 1501: Part 1: 1964 and that edition’s addenda. It was replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Those successor designations are not automatic aliases for the 1980 type-and-grade names. Name the edition or successor standard required on the purchase order.
The chemical and tensile figures below follow BS 1501-1:1980 as tabulated for this designation, including a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 values. BS 1501-2 (alloy plates) and BS 1501-3 (corrosion- and heat-resisting plates, sheet and strip) are different parts of the same historical series.
SHH STEEL produces and exports BS 1501-224 Grade 490B plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.
Material specification for BS 1501-224 Grade 490B
The items below follow BS 1501-1:1980. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.
| Parameter | Detail |
|---|---|
| Standard | BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates |
| Official designation | BS 1501-224 Grade 490B |
| Steel type | Fully killed aluminium-treated carbon-manganese steel |
| Product form | Hot-rolled steel plate (this part does not cover bars, sections, forgings, tubes or stainless sheet) |
| How designations are listed | Type number, tensile grade and suffix A or B; optional LT or RT impact suffixes where Table 1 allows; optional L after types 223, 224 and 225 when nickel is limited to 0.30 % |
| Applicable thickness | Up to and including 150 mm in the 1980 tensile table |
| Usual heat treatment | Normalized, unless an alternative condition is agreed. |
| Chemical analysis | Ladle analysis as tabulated for this type and grade in BS 1501-1:1980 |
| Tensile properties | Yield strength, tensile strength and elongation, by thickness, from that edition |
| Our supply | We produce and export 224 Grade 490B plate to the ordered edition, delivery condition, dimensions and extra tests |
Chemical composition of BS 1501-224 Grade 490B
The figures below are ladle analysis for BS 1501-224 Grade 490B from BS 1501-1:1980. Values are in weight percent.
| Element | 224 Grade 490B ladle analysis, BS 1501-1:1980 (wt. %) |
|---|---|
| Carbon (C) | 0.22 max |
| Silicon (Si) | 0.10–0.40 |
| Manganese (Mn) | 0.90–1.60 |
| Phosphorus (P) | 0.030 max |
| Sulfur (S) | 0.030 max |
| Aluminium, metallic (Al) | 0.015 min |
| Chromium (Cr) | 0.25 max |
| Copper (Cu) | 0.30 max |
| Molybdenum (Mo) | 0.10 max |
| Nickel (Ni) | 0.75 max |
Figures are ladle analysis as tabulated for this designation in BS 1501-1:1980. Determination of total aluminium is deemed to meet the metallic aluminium requirement when the value obtained is not less than 0.018 %. The combined total of chromium, copper and molybdenum is 0.50 % maximum. A suffix L may be added after the type number when a maximum nickel content of 0.30 % is specified; in that case the combined total of chromium, copper, molybdenum and nickel is 0.70 % maximum. Nitrogen shall not exceed 0.012 %. The 1980 edition allows the purchaser to specify tighter phosphorus and sulfur limits. Elevated-temperature numerical values for suffix B belong in Appendix F and should be taken from the edition named on the order.
Tensile and related properties for BS 1501-224 Grade 490B
224 Grade 490B has thickness-dependent yield strength, tensile strength and elongation. Values below are from BS 1501-1:1980. Strength values are in N/mm², equivalent to MPa.
| Thickness | Tensile strength Rm, N/mm² | Yield strength Re, N/mm² min | Elongation A, % min |
|---|---|---|---|
| Over 3 mm up to and including 16 mm | 490–610 | 325 | 21 |
| Over 16 mm up to and including 40 mm | 490–610 | 315 | 21 |
| Over 40 mm up to and including 63 mm | 490–610 | 305 | 20 |
| Over 63 mm up to and including 100 mm | 490–610 | See note | 19 |
| Over 100 mm up to and including 150 mm | 490–610 | See note | 19 |
For thickness greater than 63 mm, the 1980 tensile table states that the minimum yield strength is the 40 mm to 63 mm value reduced by 1 % for each 5 mm increase over 63 mm. Those thicker yields are not recalculated here. The room-temperature yield and elongation bands are the same as those tabulated for 224 Grade 460; the tensile window for this grade is 490–610 N/mm² as stated for grade 490 in BS 1501-1:1980. If specified, Charpy V-notch values for type 224 plates up to and including 80 mm thick apply to all type 224 grades as tabulated below from that edition. Values for plates over 80 mm thick shall be agreed at enquiry.
Minimum average Charpy V-notch energy for type 224 plates up to and including 80 mm thick, all grades, from BS 1501-1:1980.
| Test temperature | Minimum average of three, J |
|---|---|
| Room temperature (RT) | 61 |
| 0 °C (LT0) | 55 |
| −20 °C (LT20) | 47 |
| −30 °C (LT30) | 41 |
| −40 °C (LT40) | 31 |
| −50 °C (LT50) | 27 |
Suffix B specifies characteristic elevated-temperature yield or 0.2 % proof-stress values in the 1980 appendices. Those high-temperature figures should be taken from the edition named on the order.
Delivery conditions for BS 1501-224 Grade 490B
Type 224 is supplied as fully killed aluminium-treated carbon-manganese steel plate. The 1980 text specifies normalized supply unless an alternative condition is agreed. Name the required delivery condition on the purchase order.
If the project has moved to EN 10028-2 or EN 10028-3, order the successor designation and edition expressly. A later name is not by itself a substitute instruction.
The purchase order should name the official designation including the A or B suffix, any required impact suffix, thickness, width and length, the delivery condition, any extra tests, and the inspection document required.
This page does not offer heat-treatment or fabrication services.
Welding and thermal cutting
BS 1501-1:1980 does not set a welding procedure. Type 224 is an aluminium-treated carbon-manganese vessel plate intended for welded pressure equipment. Welding and thermal cutting should be qualified for the carbon content, thickness and delivery condition.
Heat input and any required post-weld heat treatment belong in the project specification.
Form, appearance, dimensions and thickness tolerances
Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate tolerances when that standard is specified.
Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.
Applications and specification limits
We produce and export 224 Grade 490B plate as fully killed aluminium-treated carbon-manganese steel plate for fired and unfired pressure equipment. Typical service includes welded boilers and vessels that specify type 224 grade 490B. The 1980 clauses cover type 224 plates up to 150 mm in grades 400, 430, 460 and 490. This page specifies grade 490 only.
BS 1501-1:1980 is a historical carbon and carbon-manganese plate standard for pressure purposes. It is not the current EN 10028-2 or EN 10028-3 order unless that successor standard is written on the enquiry, and it is not a BS 1501-2 alloy, BS 1501-3 stainless, BS 1502 bar or BS 1503 forging order.
Compare BS 1501-224 Grade 490B with other steel plates
224 Grade 490B is a BS 1501-1:1980 pressure-vessel plate. The comparison below is for selection only; these materials are not equivalents.
| Material | Alloy / type | Delivery condition | Mechanical requirements | Typical service | Substitution limit |
|---|---|---|---|---|---|
| BS 1501-224 Grade 490B (this plate) | BS 1501-1:1980 official designation | Normalized, unless an alternative condition is agreed. | Yield 325 N/mm² minimum up to 16 mm; tensile 490–610 N/mm², with suffix B elevated-temperature properties | Typical service includes welded boilers and vessels that specify type 224 grade 490B | A different standard, later EN name, or 1980 type is not an automatic substitute |
| BS 1501 224 Grade 490A steel plate | BS 1501-1:1980 official designation | Normalized, unless an alternative condition is agreed. | Yield 325 N/mm² minimum up to 16 mm; tensile 490–610 N/mm² | Same type and tensile grade without specified elevated-temperature values | A different 1980 suffix, not an automatic substitute |
| EN 10028-3 P355NH | Weldable fine-grain elevated-temperature vessel plate, steel number 1.0565 | As specified in EN 10028-3 | Published yield 355 MPa and tensile 490–630 MPa | Modern European fine-grain boiler and vessel plate | Related aluminium-treated / fine-grain class only |
| EN 10028-2 P355GH | Non-alloy elevated-temperature vessel plate, steel number 1.0473 | As specified in EN 10028-2 | Published yield 355 MPa and tensile 510–650 MPa | Modern European carbon-manganese boiler and vessel plate | Related product form only |
| ASTM A516 Grade 70 | Carbon steel pressure-vessel plate, offered here as a normalized-product comparison. | Normalized plate is described on the linked product page; specify the actual ordered condition. | Use its own ordered specification, thickness and delivery condition; no strength or toughness value is transferred to this grade. | Welded pressure vessels and storage equipment in moderate- and lower-temperature service. | Different standard and acceptance rules; BS type, deoxidation practice and A/B elevated-temperature suffix are not carried into the ASTM name. Strength, impact testing and design approval must be checked under the actual order. |
Equivalent and related grades by country
The designations below are near names, not automatic substitutes. A later EN 10028 designation does not by itself authorize substitution. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form.
| Country / region | Standard | Grade or designation | Similarity and key differences | Substitution caveat |
|---|---|---|---|---|
| United Kingdom (this plate) | BS 1501-1:1980 | 224 Grade 490B | Same ladle analysis and room-temperature tensile window as 224 Grade 490A, with specified elevated-temperature values in Appendix F. Grade 490 is treated differently from the other type 224 grades in the 1980 elevated-temperature verification rule. Product form is plate up to 150 mm. | This product |
| Europe | EN 10028-3 | P355NH (1.0565) | Related fine-grain vessel plate with specified elevated-temperature properties. Live product states yield 355 MPa and tensile 490–630 MPa. | Near name only. |
| Europe | EN 10028-2 | P355GH (1.0473) | Related C-Mn vessel plate. Live product states yield 355 MPa and tensile 510–650 MPa. | Related product form only. |
| United States | ASTM A516/A516M | Grade 70 | Related carbon vessel plate. Live product states yield 260 MPa and tensile 485–620 MPa. | Related product form only. |
Why choose SHH STEEL for BS 1501-224 Grade 490B
- We produce and export BS 1501-224 Grade 490B pressure-vessel steel plate
- We review the enquiry for edition, designation, delivery condition, dimensions and extra tests
- We keep the 1980 type, tensile grade and A/B suffix distinct from later EN 10028 names and from BS 1501-2 / BS 1501-3
- We match documentation to what the purchase order requires
How to enquire for BS 1501-224 Grade 490B plate
| Item | What to specify |
|---|---|
| Standard and designation | BS 1501-224 Grade 490B and the edition required |
| Or successor standard | EN 10028-2 or EN 10028-3 designation and edition, if that is what the project now requires |
| Delivery condition | Normalized, unless an alternative condition is agreed. |
| Dimensions | Required thickness, width and length |
| Chemistry | Ladle analysis to BS 1501-1:1980, or to another named edition |
| Mechanical tests | Yield strength, tensile strength, elongation and, where specified, elevated-temperature or impact tests to the named edition |
| Other tests | Ultrasonic examination or other extra tests only when written on the order |
| Documentation | State the inspection document type required by the project |
Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.
FAQ
-
Is BS 1501 still a current product standard?
- No. BS 1501-1:1980 is the last final edition of Part 1. It was withdrawn on 15 February 1993 and replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Projects still using the 1980 designation should name that edition on the order.
-
Which edition do the tables on this page follow?
- They follow BS 1501-1:1980, including tabulated values from a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 tables. Specify the edition or successor standard required on the purchase order.
-
Does BS 1501-1 cover alloy or stainless pressure-vessel plates?
- No. Part 1 covers carbon and carbon-manganese plates. Alloy plates belong to BS 1501-2:1988. Corrosion- and heat-resisting plates, sheet and strip belong to BS 1501-3:1990. Bars and sections belong to BS 1502, and forgings to BS 1503. This page is 224 Grade 490B only.
-
Can P355NH be used instead of 224 Grade 490B?
- Only after a project review. Live P355NH is stated as 355 MPa yield and 490–630 MPa tensile, against 325 N/mm² and 490–610 N/mm² for 224 Grade 490. Suffix B elevated values remain those of BS 1501-1:1980 Appendix F; grade 490 follows a different elevated-temperature verification rule from the other type 224 grades.
-
What should a quotation enquiry include?
- BS 1501-224 Grade 490B, the edition required or the successor designation, the delivery condition, plate thickness by width by length, quantity, any extra tests, and the inspection document required.
Request a quotation
Contact SHH STEEL for a quotation for BS 1501-224 Grade 490B steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.
Specify the edition (BS 1501-1:1980 or a named successor such as EN 10028-2 or EN 10028-3), the A or B suffix, any required impact suffix, the delivery condition and any specimen heat treatment. If your project requires ultrasonic examination, a stated impact temperature or another extra test, include the acceptance criteria and the inspection document required.
If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.
Contact: admin@steelspecs.com