ASTM A240 UNS S41008 Stainless Steel Sheet
What is ASTM A240 UNS S41008 stainless steel sheet?
Type 410S is the low-carbon (≤ 0.08 %) 12 % chromium grade, designed to stay soft and ductile after welding or cooling from high temperature. Thin 410S sheet is common as a lining material and in heat-resisting parts. Ferritic grades are produced mostly as sheet and strip, because their toughness is best in thin gauges. They are magnetic, contain little or no nickel, and hold a stable price, which is why they dominate appliances, exhaust systems and indoor trim. Under ASTM A480, “sheet” means flat material under 5.00 mm thick and at least 600 mm wide, and narrower cold-rolled material is strip. That makes UNS S41008 (Type 410S) sheet a cold-rolled or thin hot-rolled product with its own finish, gauge-tolerance and flatness rules, quite different from plate. S41008 sheet is a regular mill product, so most thicknesses and finishes can be supplied from current production or stock.
This guide covers S41008 sheet from the buyer’s side of the order: the A240 and A480 requirements, heat and product analysis, properties, cold-rolled finishes, gauge and flatness tolerances, coil and cut-length supply, equivalent EN, JIS and GB/T grades, and the certificates to expect. SHH STEEL supplies S41008 sheet and coil mill-direct and can slit, cut and protect it to your drawings.
SHH STEEL quotes every value here from the standard named beside it; where a standard leaves a point to agreement, this page says so.
UNS S41008 (Type 410S) sheet: specification summary
ASTM A240/A240M sets the chemistry and properties for UNS S41008 (Type 410S), and ASTM A480/A480M supplies the general rules for flat products: definitions, finishes, tolerances, testing and marking. A240 is written for general and pressure applications. Its ASME twin, SA-240, matters only when the sheet goes into ASME Code equipment, so most sheet for appliances, architecture, transport and process equipment is simply ordered to A240.
| Property | A240 sheet data for UNS S41008 |
|---|---|
| Standard | ASTM A240/A240M, chromium and chromium-nickel stainless steel plate, sheet and strip |
| General requirements | ASTM A480/A480M: ordering, finishes, tolerances, product analysis, testing, marking |
| ASME counterpart | ASME SA-240 is the Code adoption; order SA-240 only when the sheet is for ASME Code construction |
| UNS number | UNS S41008 |
| Type name | Type 410S |
| Structure | ferritic (body-centred cubic) |
| Sheet (A480 3.2.3) | under 5.00 mm thick and 600 mm and over wide |
| Strip (A480 3.2.4) | cold-rolled, under 5.00 mm thick and under 600 mm wide |
| Typical gauges | Cold-rolled coil and sheet about 0.3–3.0 mm (to 4 mm on some lines); hot-rolled sheet and coil from about 3 mm up to the 5.00 mm sheet limit |
| Typical widths | 1000, 1219, 1250 and 1500 mm; other widths by slitting |
| Supply forms | coil, slit coil, cut-to-length sheet, blanks cut to size |
| Condition | Heat treated so that all mechanical and bend requirements of A240 Table 2 are met; A480 15.4.1 does not fix a single temperature for these chromium steels |
| Cold-rolled finishes | 2D, 2B, BA; No.3, No.4, No.6, No.7, No.8; hairline (HL) by agreement; No.1 for hot-rolled sheet |
| Dimensional tolerances | A480 Annex A2 (inch-pound) or Annex A3 (A480M), e.g. Table A3.5 thickness and A3.8 flatness for cold-rolled wide sheet |
| Required tests | heat analysis; tension test and hardness; 180° bend |
| Optional tests | PMI, Charpy (S1 where applicable), as agreed |
| Marking | specification, type or UNS, heat/identification number and producer; coils marked near the outside end plus inside tag; sheet under 6.4 mm is not die-stamped |
| Certificates | mill test report per A480 Section 8; EN 10204 3.1 as standard; 3.2 with third-party witness on request |
This grade sits in the ASTM A240 UNS sheet and plate range and the wider ASTM A240/A240M range. Where A480 and A240 conflict, A240 governs, and a stricter purchase-order requirement governs both, but an order cannot waive a required test. Name A240M on the order if you want metric tolerances from A480 Annex A3.
UNS S41008 sheet chemistry: heat analysis vs product analysis
Heat analysis limits for UNS S41008 (Type 410S), in percent by mass (maximum unless a range or minimum is shown), from ASTM A240 Table 1:
| Grade | C | Mn | P | S | Si | Cr | Ni |
|---|---|---|---|---|---|---|---|
| UNS S41008 | 0.08 | 1.00 | 0.040 | 0.030 | 1.00 | 11.5–13.5 | 0.60 |
Two different analyses can appear in a sheet purchase. The heat analysis is the steelmaker’s analysis of the melt, taken during pouring or from in-process product. It is the analysis printed on the mill certificate, and it must sit inside Table 1 (A480 6.2). The product analysis is a check the buyer may make on finished sheet or coil to confirm identity (A480 7.1). Because a thin cold-rolled product can show small local variation, A480 Table A1.1 allows product analysis to fall slightly outside Table 1. The comparison below applies those tolerances to S41008:
| Element | Heat analysis, % (ASTM A240 Table 1) | A480 Table A1.1 tolerance | Product analysis limit, % |
|---|---|---|---|
| Carbon (C) | 0.08 max | 0.01 over max | ≤ 0.09 |
| Manganese (Mn) | 1.00 max | 0.03 over max | ≤ 1.03 |
| Phosphorus (P) | 0.040 max | 0.005 over max | ≤ 0.045 |
| Sulfur (S) | 0.030 max | 0.005 over max | ≤ 0.035 |
| Silicon (Si) | 1.00 max | 0.05 over max | ≤ 1.05 |
| Chromium (Cr) | 11.5–13.5 | 0.15 under min / 0.15 over max | 11.35–13.65 |
| Nickel (Ni) | 0.60 max | 0.03 over max | ≤ 0.63 |
The tolerance band is picked by the specified limit, or by the top of a range, and applies below a minimum and above a maximum. Results for one element across several samples of a heat must not straddle the range, falling both above and below it (A480 7.2). For ratio requirements such as Ti ≥ 5×(C+N), product analysis must reach at least 0.90× the ratio (A480 A1.1). Limits on unspecified Cu, Mo, Ti and Nb (0.75, 0.75, 0.10 and 0.10 %) stop sheet of one grade being certified when it actually matches another (A480 6.3.1).
A practical note for receiving inspection: handheld XRF identifies the alloy family but cannot measure carbon or nitrogen. So it cannot tell 304 from 304L, or a standard grade from an H or N grade. Use spark-OES or a laboratory analysis when those elements decide acceptance.
Role of the main elements in S41008 sheet:
- Carbon ≤ 0.08 %: a standard carbon level. Keep holding time in the sensitising range short when corrosion resistance after welding matters.
- Chromium 11.5–13.5 %: forms the passive film that makes the steel stainless; higher chromium improves resistance to corrosion and oxidation.
Mechanical properties of S41008 sheet
Annealed room-temperature requirements from ASTM A240 Table 2:
| Condition / thickness | Tensile strength, min | Yield strength 0.2 %, min | Elongation in 50 mm, min | Hardness, max | Cold bend |
|---|---|---|---|---|---|
| All thicknesses | 415 MPa [60 ksi] | 205 MPa [30 ksi] | 22 % (20 at ≤ 1.27 mm) | 183 HBW / 89 HRBW | 180° |
For thin sheet, A240 lowers the elongation minimum to 20 % at 1.27 mm and under (Table 2 note N).
For coil product, A480 16.1.1 requires at least two hardness tests (one from each end), one bend test when required, and one or more tension tests from each coil. If the hardness at the two ends differs by more than 5 HRB, or the coil is temper rolled, tensile properties are determined at both ends. Cut-length sheet is tested per lot of 100 pieces or fewer of the same heat, thickness and heat-treatment run (16.1.2).
Hardness on thin sheet may be measured by an alternative method suited to the gauge, with conversions per A370. When sheet is too thin for any Rockwell superficial test, the hardness requirement is waived (A480 17.2.1).
Bend specimens from sheet are full thickness and about 25 mm wide (A480 17.3.2). Sheet up to 9.5 mm is bent over flat stock of its own thickness (1T), and the outside of the bend must show no cracks (17.4.1).
Cold-rolled finishes for S41008 sheet: 2B, BA, No.4, HL and more
For sheet, finish often matters as much as chemistry because it decides appearance, cleanability and how the part forms. A480 Section 11 lists the sheet finishes below, and all are available on S41008 subject to the mill route:
| Finish | Description (A480 Section 11 and Note 3) | Typical sheet use |
|---|---|---|
| No. 1 | Hot-rolled, annealed and descaled; dull and non-reflective | Hot-rolled sheet, heat-resisting and industrial parts |
| No. 2D | Cold-rolled, dull; smooth, non-reflective and non-directional, holds lubricant in deep drawing | Deep-drawn and severely formed parts |
| No. 2B | Cold-rolled, bright; smooth, moderately reflective, from a final light pass on polished rolls; polishes more readily than No. 1 or 2D | General-purpose sheet; the standard mill finish |
| BA (bright annealed) | Smooth, bright, reflective; cold rolled then annealed in a protective atmosphere to prevent scaling | Appliance panels, reflectors, hygienic and decorative parts |
| No. 3 | Intermediate polish, linear texture; Ra generally up to 40 µin (about 1.0 µm) | Pre-polished sheet for further finishing |
| No. 4 | General-purpose polish, linear texture; Ra generally up to 25 µin (about 0.6 µm) | Kitchen, architectural and elevator panels |
| No. 6 | Dull satin, produced by Tampico brushing a No. 4 finish | Architectural and decorative work |
| No. 7 | High lustre, buffed from a finely ground surface with grit lines still present | Ornamental and architectural parts |
| No. 8 | Mirror; polished with successively finer abrasives and buffed | Mirrors, reflectors, signage |
| TR | Cold-worked to obtain specified properties | Springs and high-strength formed parts |
| HL (hairline) | Commercial long-line brushed finish; not defined in A480, so it is agreed by description or sample | Elevators, doors, interior panels |
Polished sheet can be ordered polished on one side or both; when only one side is polished, the other side may be rough ground to get flatness (A480 11.1.12). Architectural finishes, sometimes called No. 5, and special textures are negotiated between buyer and seller. A480 Note 3 is guidance, not a basis for rejection, so agree a reference sample for any decorative finish. Laser-grade PVC film, paper interleaving and grain direction should be stated on the order when the face side matters.
Gauge, width, length and flatness tolerances for S41008 sheet
Gauge and flatness tolerances come from A480 Annex A3 for A480M (metric) orders and Annex A2 for inch-pound orders. For cold-rolled wide coil and cut lengths, Table A3.5 gives these thickness tolerances, over and under:
| Specified thickness, mm | w ≤ 1000 mm | 1000 < w ≤ 1300 mm | 1300 < w ≤ 2100 mm |
|---|---|---|---|
| 0.30 | ± 0.03 | — | — |
| 0.40 | ± 0.04 | ± 0.04 | — |
| 0.50 | ± 0.045 | ± 0.05 | — |
| 0.60 | ± 0.05 | ± 0.05 | — |
| 0.80 | ± 0.05 | ± 0.05 | — |
| 1.00 | ± 0.055 | ± 0.06 | ± 0.07 |
| 1.20 | ± 0.08 | ± 0.08 | ± 0.08 |
| 1.50 | ± 0.08 | ± 0.08 | ± 0.10 |
| 2.00 | ± 0.10 | ± 0.10 | ± 0.11 |
| 2.50 | ± 0.10 | ± 0.11 | ± 0.13 |
| 3.00 | ± 0.13 | ± 0.13 | ± 0.15 |
| 4.00 | ± 0.17 | ± 0.17 | ± 0.17 |
Thickness is measured at least 15 mm from a slit edge or 25 mm from a mill edge. For a thickness between two rows, the next higher row applies. Some mills roll tighter than the table, and a tighter tolerance can be agreed on the order. Order thickness as a decimal or fraction, not a gauge number; under A480 4.1.7 the gauge number is not a basis for rejection.
Width tolerance for cut lengths and coil is plus-only (Table A3.6, selected rows):
| Specified thickness, mm | 600 < w ≤ 1000 mm | 1000 < w ≤ 2100 mm |
|---|---|---|
| 1.00 | +1.5 / −0 | +2.0 / −0 |
| 1.50 | +1.5 / −0 | +2.0 / −0 |
| 2.50 | +2.0 / −0 | +2.5 / −0 |
| 3.50 | +3.0 / −0 | +3.0 / −0 |
Length tolerance for cut lengths (not resquared) is +5 / −0 mm up to 2000 mm and +0.0025 × L / −0 above 2000 mm (Table A3.7). Flatness is the maximum deviation from a horizontal flat surface (Table A3.8):
| Flatness standard | Thickness / width / length | Max. deviation from a flat surface |
|---|---|---|
| Not stretcher-levelled | width under 1500 mm (any thickness) | 10 mm |
| Not stretcher-levelled | width 1500 mm and over | 12 mm |
| Stretcher-levelled | t ≤ 4.99 mm, w < 1200 mm, L < 2400 mm | 4 mm |
| Stretcher-levelled | t ≤ 4.99 mm, other width/length combinations | 7 mm |
The Table A3.8 values exclude hard tempers of 2xx and 3xx grades, dead-soft and deep-drawing sheet, which have their own rules. If panels will be laser cut, bonded or used as visible cladding, order stretcher-levelled flatness or a tighter flatness by agreement.
S41008 coil, slit coil and cut-to-length sheet supply
S41008 is supplied in four forms. Coil is the mill product, supplied at full width. Slit coil is cut to narrower widths; under 600 mm wide it becomes strip, ordered with edge No. 1 (rolled), No. 3 (slit) or No. 5 (square after slitting) per A480 Section 14. Cut-to-length sheet is levelled and sheared to length, and blanks are cut to drawing.
For coils, state the inside diameter your decoiler takes (often 508 or 610 mm) and the maximum coil weight. Coils are marked near the outside end, with an inside tag carrying the same data (A480 25.1.1.3), and packaging follows ASTM A700 unless the order says otherwise (A480 25.1.2).
SHH STEEL can slit, cut to length, level, apply protective film and pack S41008 sheet in its own workshop, so you receive sizes ready for your laser, press brake or production line.
Annealing and heat treatment of S41008 sheet
A480 condition for UNS S41008 (Type 410S): heat treated so that all mechanical and bend requirements of A240 Table 2 are met; A480 15.4.1 does not fix a single temperature for these chromium steels.
Sheet is annealed on continuous annealing and pickling lines, or in a protective-atmosphere line for BA finish. The heat treatment must be a separate cycle and cannot be replaced by an in-process thermal cycle (A480 15.1). Material that fails a test may be re-heat-treated and retested (A480 20.5).
How S41008 sheet performs in service
Ferritic sheet is not prone to chloride stress-corrosion cracking, and its corrosion resistance rises with chromium and molybdenum. Titanium and niobium stabilisation protects weld zones and improves weld ductility. Long exposure in about the 400–540 °C range can cause 475 °C embrittlement, which limits use for long-term loaded service in that band.
S41008 sheet equivalents: ASTM, EN, JIS and GB/T compared
Buyers often send drawings that name an EN, JIS or GB grade rather than UNS S41008 (Type 410S). The table shows the nearest cross-references for sheet. “Nearest” means the grades share the same metallurgical concept, not that they are interchangeable on a certificate. SHH STEEL checks each element and each property against every standard named on the enquiry before offering dual certification.
| System | Sheet standard | Grade | How close | Notes for sheet buyers |
|---|---|---|---|---|
| ASTM | A240 with A480 | UNS S41008 (Type 410S) | reference | State the edition and A240 or A240M |
| EN | EN 10088-2 (also EN 10088-4, EN 10028-7) | 1.4000 X6Cr13 | nearest; check each limit | Proof strengths depend on product form (C = cold-rolled strip, H = hot-rolled strip, P = plate); elongation uses A80 or A gauge lengths |
| JIS | JIS G4305 (cold-rolled) / G4304 (hot-rolled) | SUS410S | nearest; check each limit | SUS grade with its own ranges; compare C, N and Ni with A240 |
| GB/T | GB/T 3280 (cold-rolled) / GB/T 4237 (hot-rolled) | 06Cr13 (S41008) | nearest; check each limit | GB/T 20878 name and code; the S-code is not a UNS number |
EN. EN 10088-2 is the main European standard for corrosion-resisting sheet, strip and plate for general purposes. Its property tables are split by product form: cold-rolled strip (C), hot-rolled strip (H) and hot-rolled plate (P). A thin cold-rolled sheet is therefore checked against the C-row values for its thickness. EN 10088-4 covers sheet and strip for construction, and EN 10028-7 covers flat stainless products for pressure equipment. EN tensile tests report 0.2 % and 1 % proof strength, and thin-sheet elongation is measured on an 80 mm gauge length, so the numbers do not convert one-for-one to the A240 50 mm elongation. See the EN 10088-2 stainless range for related steel numbers.
JIS. JIS G4305 covers cold-rolled stainless plate, sheet and strip, which includes most thin sheet, and JIS G4304 covers the hot-rolled product. SUS grades follow the AISI-type concept but their ranges are set independently. Japanese-specified sheet should be checked for carbon, nitrogen and nickel against the A240 row. The JIS G4305 range lists the SUS sheet grades.
GB/T. Chinese cold-rolled sheet is ordered to GB/T 3280 and hot-rolled sheet to GB/T 4237, with grade names and numeric codes from GB/T 20878. A code such as S30408 is a Chinese designation, not a UNS number, so certificates must state which standard the code belongs to. See the GB/T 4237 range for related Chinese grades.
Other ASTM and ASME specifications. A480 supplies the general rules for A240 sheet. SA-240 is the ASME Code adoption of A240 and is needed only for ASME Code equipment. Other product forms in the same UNS grade, such as pipe, tube and bar, have their own ASTM specifications, so check each one when you need a matching set.
Other A240 sheet grades related to S41008
Sheet buyers comparing S41008 usually look at these grades in the same A240 sheet series:
- ASTM A240 UNS S41000 stainless steel sheet
- ASTM A240 UNS S40920 stainless steel sheet
- ASTM A240 UNS S43000 stainless steel sheet
For the same material in other product forms and designations, see ASME SA240 UNS S41008 stainless steel plate, ASTM A240 Type 410S sheet and plate, AISI 410S stainless steel. Those pages cover plate or type-designation ordering, while this page covers thin sheet and coil.
More grades and standards are listed in the stainless steel sheets and plates pages.
S41008 sheet applications, forming and welding
Typical uses of S41008 sheet and coil:
- Refinery and petrochemical liners
- Heat-treatment boxes and furnace parts
- Automotive and appliance parts
- Clad and lining sheet
Ferritic sheet bends and stretch-forms well in thin gauges and has lower work-hardening than austenitic sheet, though it is less suited to very deep draws. Weld with low heat input to limit grain growth; stabilised grades keep welds more ductile.
Keep the protective film on during laser cutting and forming. Keep sheet away from carbon-steel dust and tools, because embedded iron rusts and spoils the finish, and pickle or passivate welds where appearance or corrosion resistance matters.
Certificates, testing and receiving inspection for S41008 sheet
Every S41008 sheet delivery from SHH STEEL comes with the original mill test report. Under A480 8.1, it names the specification and year, the grade or grades, the heat analysis and the required test results. A supplier that is not the mill must pass on a copy of the original manufacturer’s report (A480 8.4). EN 10204 3.1 is standard, and 3.2 with witness by TUV, ABS, CCS, BV, DNV, LR or your own inspector can be arranged.
On receipt, match the marking to the certificate, measure thickness at the A480 positions, check flatness and finish, and run PMI where required. Test-based rejections must be reported within 60 working days of receipt (A480 23.1).
Sourcing S41008 sheet: buyer concerns and SHH STEEL solutions
These are the questions sheet buyers ask SHH STEEL most often, and how we handle each one:
| Buyer Concern | SHH STEEL Solution |
|---|---|
| Fake material or certificates | Coils and sheet lots can be witnessed by TUV, ABS, CCS or another class society, and partner laboratories run PMI, chemistry and tensile checks against the order. Third-party witness and EN 10204 3.2 certificates available. |
| Unsafe deposit | TT and LC are accepted, including TT + LC splits. For large projects you can sign directly with the mill, with SHH STEEL coordinating documents and follow-up for a small service fee. |
| Small orders below mill MOQ | Small sheet quantities are consolidated with other customers’ orders of the same grade, thickness and finish, so lots below the mill MOQ still come from genuine mill coils with full traceability. |
| Slow delivery | Dedicated staff chase the mill schedule through cold rolling, annealing, finishing and slitting, and report progress at each stage. |
| Processing needs | Our own workshop handles cutting to size, bevelling, machining to drawings and surface pretreatment such as film protection, so sheets arrive ready to fabricate. |
How to order UNS S41008 sheet from SHH STEEL
A480 4.1 puts the responsibility for a complete order on the buyer. For S41008 sheet, include:
- Quantity by weight and number of sheets or coils.
- Specification and edition: ASTM A240 or A240M, plus any second standard for dual certification.
- Grade: UNS S41008 (Type 410S).
- Condition and finish, for example annealed 2B, BA, or No.4 on one side with film.
- Form and dimensions: thickness, width and length in the same units, or coil ID, OD and weight; strip edge type if slit.
- Tolerances or flatness tighter than A480, if needed.
- Tests and documents: PMI, corrosion or phase tests, EN 10204 3.1 or 3.2, inspector, marking and packing.
SHH STEEL combines mill-direct sourcing with its own processing workshop. We check your grade and finish choice, offer dual certification when a heat qualifies, consolidate small quantities, follow the mill schedule and cut or slit before shipment. TT and LC payment are accepted.
Send your S41008 sheet enquiry with sizes, finish and quantity. The SHH STEEL team will reply with a quotation, lead time and inspection plan.
FAQ
-
What is 410S sheet used for?
- Mainly linings, furnace parts and general fabrications that need 12 % chromium steel without hardening after welding. It is also used as a low-cost oxidation-resistant sheet in mild heat service.
-
What elongation does thin 410S sheet need?
- A240 sets 22 % minimum elongation, reduced to 20 % for sheet 1.27 mm and thinner. Its 180° bend test still applies to the sheet.
-
Can 410S sheet be hardened?
- Not significantly. Its low carbon means it develops little hardness after cooling, unlike Type 410.
-
Can I buy S41008 stainless steel sheet cut to size in small quantities?
- Yes. SHH STEEL consolidates small S41008 sheet orders with other customers’ orders of the same grade and finish, and cuts sheets or blanks to size in its own workshop. That way small lots still come from traceable mill coils.
-
What thickness tolerance applies to cold-rolled S41008 sheet?
- For A480M orders, Table A3.5 applies. For example, 1.00 mm sheet up to 1000 mm wide is allowed ±0.055 mm, and 2.00 mm sheet ±0.10 mm. Tighter tolerances can be agreed on the order.
-
Which certificate comes with A240 S41008 sheet?
- Each delivery carries the original mill test report to A240 and A480, normally as EN 10204 3.1. Third-party witness and EN 10204 3.2 certificates can be arranged with TUV, ABS, CCS or another inspector.
Conclusion
ASTM A240 UNS S41008 Stainless Steel Sheet is bought for its combination of chemistry, finish and gauge accuracy, so the order should define all three: the A240 edition and UNS number, the finish and protective film, and the A480 tolerance or flatness level. SHH STEEL supplies S41008 sheet and coil from mill partners, cut or slit to your needs, with certificates you can check line by line.