ASME SA-36 S Shape I Beams

ASME SA-36 S-shape I-beams are carbon structural American Standard Beams as printed in ASME BPVC Section II, Part A, 2023. That text is identical with ASTM A36/A36M-19 and covers shapes, plates and bars. Yield is 36 ksi (250 MPa) with 58-80 ksi tensile strength. An A36 S-shape certificate is not SA-36. SHH STEEL reviews the Code edition and certificate before quoting.
Keywords
ASME SA-36 S Beam, SA-36 American Standard Beam, SA-36 S-shape, SA-36 S24x121, BPVC SA-36 I-beam
Equivalent Grades:
Near-equivalents only, not automatic substitutes.
Share:
General Description
Material Specification
Available Sizes of ASME SA-36 S Shape I Beams
Chemical Composition
Mechanical Properties
Applications
Equivalent Grades
Sourcing
FAQ
Conclusion

What are ASME SA-36 S Shape I Beams?

ASME SA-36/SA-36M, as printed in ASME BPVC Section II, Part A, 2023, is marked identical with ASTM Specification A36/A36M-19. Scope 1.1 covers carbon steel shapes, plates and bars. This page is for American Standard S-shapes only. It is not the live ASTM A36 S-shape page, not an SA-36 bar page, and not an SA-36 wide-flange, angle or channel page.

An ordinary ASTM A36 S-shape certificate is not an SA-36 certificate. The SA designation is used when the order needs the ASME materials listing. The Code edition on the order governs; a later ASTM A36 year is not automatically the SA text in the 2023 book.

Material, Dimensions and Tolerances for ASME SA-36 S Shapes

The steel shall be killed. Structural products shall conform to the current edition of Specification A6/A6M for the product ordered, unless a conflict exists, in which case SA-36 prevails. The chemistry below is the shapes column of Table 3, not the bar columns used on the SA-36 bar page. The standard S series tabulated here has a maximum flange thickness of 1.09 in, so the over-3 in wide-flange manganese and silicon notes do not apply to these 28 designations.

ASME SA-36 S Shape Sizes: American Standard Beams (ASTM A6/A6M)

The table lists the same 28 typographical A6/A6M S designations already verified on the ASTM A36 S-shape page, from S24x121 to S3x5.7. The difference is the ASME listing, not a second set of designations. The table is not a mill rolling list and not a W-shape table.

Swipe horizontally to view all dimensions.

Designation d (in) bf (in) tw (in) tf (in) d (mm) bf (mm) tw (mm) tf (mm) Mass (lb/ft) Mass (kg/m) SI designation
S24×121 24.5 8.05 0.8 1.09 622 204 20.3 27.7 121 180 S610×180
S24×106 24.5 7.87 0.62 1.09 622 200 15.7 27.7 106 158 S610×158
S24×100 24 7.25 0.745 0.87 610 184 18.9 22.1 100 149 S610×149
S24×90 24 7.13 0.625 0.87 610 181 15.9 22.1 90 134 S610×134
S24×80 24 7 0.5 0.87 610 178 12.7 22.1 80 119 S610×119
S20×96 20.3 7.2 0.8 0.92 516 183 20.3 23.4 96 143 S510×143
S20×86 20.3 7.06 0.66 0.92 516 179 16.8 23.4 86 128 S510×128
S20×75 20 6.39 0.635 0.795 508 162 16.1 20.2 75 112 S510×112
S20×66 20 6.26 0.505 0.795 508 159 12.8 20.2 66 98.2 S510×98.2
S18×70 18 6.25 0.711 0.691 457 159 18.1 17.6 70 104 S460×104
S18×54.7 18 6 0.461 0.691 457 152 11.7 17.6 54.7 81.4 S460×81.4
S15×50 15 5.64 0.55 0.622 381 143 14 15.8 50 74 S380×74
S15×42.9 15 5.5 0.411 0.622 381 140 10.4 15.8 42.9 64 S380×64

S12 to S3

The mid-range and smaller S shapes, from S12×50 to S3×5.7. 15 designations in this group.

Swipe horizontally to view all dimensions.

Designation d (in) bf (in) tw (in) tf (in) d (mm) bf (mm) tw (mm) tf (mm) Mass (lb/ft) Mass (kg/m) SI designation
S12×50 12 5.48 0.687 0.659 305 139 17.4 16.7 50 74 S310×74
S12×40.8 12 5.25 0.462 0.659 305 133 11.7 16.7 40.8 60.7 S310×60.7
S12×35 12 5.08 0.428 0.544 305 129 10.9 13.8 35 52 S310×52
S12×31.8 12 5 0.35 0.544 305 127 8.89 13.8 31.8 47.3 S310×47.3
S10×35 10 4.94 0.594 0.491 254 125 15.1 12.5 35 52 S250×52
S10×25.4 10 4.66 0.311 0.491 254 118 7.9 12.5 25.4 37.8 S250×37.8
S8×23 8 4.17 0.441 0.425 203 106 11.2 10.8 23 34 S200×34
S8×18.4 8 4 0.271 0.425 203 102 6.88 10.8 18.4 27.4 S200×27.4
S6×17.25 6 3.57 0.465 0.359 152 90.7 11.8 9.12 17.25 25.7 S150×25.7
S6×12.5 6 3.33 0.232 0.359 152 84.6 5.89 9.12 12.5 18.6 S150×18.6
S5×10 5 3 0.214 0.326 127 76.2 5.44 8.28 10 15 S130×15
S4×9.5 4 2.8 0.326 0.293 102 71.1 8.28 7.44 9.5 14.1 S100×14.1
S4×7.7 4 2.66 0.193 0.293 102 67.6 4.9 7.44 7.7 11.5 S100×11.5
S3×7.5 3 2.51 0.349 0.26 76.2 63.8 8.86 6.6 7.5 11.2 S75×11.2
S3×5.7 3 2.33 0.17 0.26 76.2 59.2 4.32 6.6 5.7 8.5 S75×8.5

Wide-flange W-shape dimensions belong on the ASTM A36 Wide Flange Beam page, not in this table. Chinese HW/HM/HN sizes belong to GB/T 11263. European IPE sizes are listed on the EN 10025-2 S235JR IPE and IPN Steel I Beams page for that material system, not as A36 S dimensions.

ASME SA-36 Chemical Composition for S Shapes (Heat Analysis)

For shapes, carbon is 0.26 % maximum at all tabulated thicknesses. Manganese has no specified requirement except that it shall be determined and reported under A6/A6M; the 0.85-1.35 % band applies only to flanges over 3 in. Phosphorus is 0.04 % maximum, sulfur 0.05 % maximum and silicon 0.40 % maximum (0.15-0.40 % only when flange thickness exceeds 3 in). Copper is 0.20 % minimum only when copper steel is specified. Do not copy the bar-column carbon split onto an S-shape order.

Swipe horizontally to view all dimensions.

Element Shapes, all thicknesses (unless noted) Notes
Carbon, max, % 0.26 Do not apply the thickness-split plate columns of Table 3 to S-shapes.
Manganese, % No requirement The heat analysis for manganese shall be determined and reported under A6/A6M. For shapes with flange thickness over 3 in [75 mm], manganese shall be 0.85-1.35%.
Phosphorus, max, % 0.04 –
Sulfur, max, % 0.05 –
Silicon, % 0.40 max For shapes with flange thickness over 3 in [75 mm], silicon shall be 0.15-0.40%.
Copper, min, % 0.20 when specified Applies only when copper steel is specified on the order.

ASME SA-36 S Shape Mechanical Properties: Yield, Tensile and Elongation

Table 2 requires 58-80 ksi [400-550 MPa] tensile strength, a 36 ksi [250 MPa] minimum yield, 20 % minimum elongation in 8 in, and 21 % minimum elongation in 2 in for shapes. The 23 % elongation belongs to the plates-and-bars column and must not be used here. The 32 ksi yield reduction is for thick plates only. Charpy testing is not required unless specified (for example A6 supplementary requirement S5 or S30).

Swipe horizontally to view all dimensions.

Property Requirement Notes for shapes
Tensile strength 58-80 ksi [400-550 MPa] The 80 ksi maximum waiver for wide-flange flanges over 3 in does not arise on the standard S series.
Yield point, min 36 ksi [250 MPa] The 32 ksi reduction is for plates over 8 in thick only. It does not apply to shapes.
Elongation in 8 in [200 mm], min 20% Shapes column of Table 2.
Elongation in 2 in [50 mm], min 21% The 23% plates-and-bars figure must not be used on an S-shape certificate.

Applications and Service Limits for ASME SA-36 S Shape I Beams

SA-36 S-shapes are used in general structural frames where an American Standard Beam is named with the ASME listing. A Section II, Part A listing is not by itself permission under every construction Code part or every pressure service. SA-36 is not SA-516. Do not treat an A36 S-shape as SA-36 unless both the marking and the certificate say so.

Near-Equivalents for ASME SA-36 S Shapes: Not Automatic Substitutes

ASTM A36/A36M-19 is the text adopted as identical in the 2023 SA-36 specification, but an A36 S-shape certificate is not automatically an SA-36 certificate. SA-36 bars use the bar chemistry columns, not the shapes column on this page. A572 Grade 50 S-shapes are a different material standard.

Sourcing ASME SA-36 S Shape I Beams from SHH STEEL

Send the S designation, the length, and the BPVC Section II, Part A edition required, and name SA-36/SA-36M explicitly. Do not use the ASTM A36 S-shape term, or an SA-36 bar or wide-flange term, for this page. Create and assign only the new ASME SA-36 I-beam child term under parent 797; do not tick the H-beam SA-36 term (519) or parent 797. SHH STEEL reviews the designation, the Code edition and the certificate before quoting.

ASME SA-36 S Shape FAQs

Is SA-36 the same as the live A36 S-shape page?
The 2023 SA-36 text is identical with A36/A36M-19, and the 28 designations are the same A6 series, but an ordinary A36 certificate is not an SA-36 certificate.
Which chemistry column applies?
The shapes column of Table 3 (carbon 0.26 % max, no manganese maximum except the over-3 in note, which does not arise on these 28 rows). Do not use the bar columns.
Is elongation 23 % in 2 in?
No. That figure is the plates-and-bars column. Shapes, including these S-shapes, use 21 % in 2 in and 20 % in 8 in.
Should this post use H-beam term 519?
No. Create the I-beam child term ASME SA-36 (asme-sa-36-steel-i-beam-profiles) under parent 797, and do not tick term 519 or parent 797.

Conclusion

ASME SA-36 S-shape I-beams follow the 2023 Section II, Part A text, identical with A36/A36M-19, and use the shapes chemistry column with 36 ksi yield and 58-80 ksi tensile strength. An A36 S-shape certificate is not SA-36. Confirm the designation, the Code edition and the certificate, and assign only the new I-beam child term.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X