API 5L X65 PSL2 Steel Plate | API 5L Pipeline Steel - SHH STEEL

API 5L X65 PSL2 Steel Plate | Line Pipe Plate PSL2

API 5L X65 PSL2 is carbon / HSLA plate for welded line pipe under API Spec 5L (46th Edition) / ISO 3183, product specification level 2. Designation L450/X65: yield 450-600 MPa, tensile 535-760 MPa, Y/T max 0.93 (D > 323.9 mm). Delivery condition ordered in the steel name (Q/M). CE and CVN are mandatory. SHH STEEL supplies X65 PSL2 plate for LSAW/HFW routes with EN 10204 3.1 (or 3.2) mill test certificates.
Equivalent Grades:
ISO 3183 L450 with delivery suffix; GB/T 21237 L450M / N / Q talk; EN ISO 3183 aligned. Sibling API 5L PSL2 pages under https://www.steelspecs.com/products-item/api-5l/. Confirm against project specs.
Heat Treatment
PSL2 steel-name suffixes: Q (quenched and tempered); M (thermomechanical rolled (TMCP)). Ordered as part of the steel name (e.g. X65M).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
PSL / toughness / sour guidance
Equivalent Material Grade
X65 PSL2 vs related grades
Why choose Us
Our Service
FAQ
Conclusion

What is API 5L X65 PSL2 steel plate?

API 5L X65 PSL2 covers plate intended for line pipe manufactured to API Spec 5L (46th Edition) / ISO 3183. PSL2 X65 is limited to Q or M delivery (no R/N). TMCP X65M plate with C max 0.12% (unless agreed) is the usual LSAW feedstock. Y/T max 0.93 supports field bending predictability.

API 5L is a pipe specification; these product pages describe plate feedstock ordered to the same grade chemistry and mechanical package for welded-pipe mills (LSAW, HFW and related). State PSL, delivery letter (PSL2), dimensions, CVN/DWTT temperature and any Annex H/G/J requirements on the purchase order.

China mill-direct supply with EN 10204 3.1 (or 3.2) MTC and optional third-party inspection. Category hubs: API 5L · Pipeline Steel Plates.

Sibling / related grades: API 5L Grade B PSL2 · API 5L X42 PSL2 · API 5L X46 PSL2 · API 5L X52 PSL2 · API 5L X56 PSL2 · API 5L X60 PSL2 · API 5L X70 PSL2 · API 5L X80 PSL2 · API 5L X65 PSL1 · API 5L X65MS · GB/T 21237 L450M.

Material Specification for API 5L X65 PSL2

Parameter Specification
Standard API Spec 5L (46th Edition) / ISO 3183; confirm ordered edition on the MTC
Grade L450 / X65 (+ delivery letter)
PSL / annex PSL2
Product form Plate for welded line-pipe manufacture (LSAW / HFW and related)
Thickness relevance Chemistry tables cited for t ≤ 25.0 mm; for t > 25.0 mm composition as agreed. Plate thickness for pipe mills typically about 6-40 mm; thicker by mill inquiry. Confirm on PO/MTC.
Width / length Per mill capability and pipe-mill nesting; cut-to-size on request
Delivery condition Q/M as ordered in steel name
Surface As-rolled or shot blasted
Edge Mill edge or cut edge
Certification EN 10204 3.1 / 3.2
Density 7.85 g/cm³

Chemical Composition of API 5L X65 PSL2 by delivery letter (heat and product analysis)

Limits below are from API 5L Table 5 for PSL2 pipe with t ≤ 25.0 mm. Values apply to heat (melt) and product analyses in one table. For t > 25.0 mm, composition shall be as agreed. Footnote letters match the standard.

Element / CE X65Q X65M
C max (%) 0.18 0.12
Si max (%) 0.45 0.45
Mn max (%) 1.70 1.60
P max (%) 0.03 0.03
S max (%) 0.01 0.01
V max (%) g g
Nb max (%) g g
Ti max (%) g g
CEIIW max 0.43 0.43
CEPcm max 0.25 0.25

Footnotes (API 5L Table 5): c unless otherwise agreed Nb+V ≤ 0.06%; d Nb+V+Ti ≤ 0.15%; g unless otherwise agreed Nb+V+Ti ≤ 0.15%; other Cu/Ni/Cr/Mo caps per footnotes e/h/i. CEIIW applies if product-analysis C > 0.12%; CEPcm if C ≤ 0.12%. Carbon-manganese trade-off footnote applies within stated caps. No intentional B (residual ≤ 0.001%) except where footnote j applies on higher grades.

Seamless pipe with t > 20.0 mm: CE limits shall be as agreed.

Mechanical Properties of API 5L X65 PSL2

API 5L Table 7 tensile requirements for PSL2 pipe body. Y/T max 0.93 applies when D > 323.9 mm (12.750 in).

Grade Yield Rt0.5 Tensile Rm Y/T max Delivery
L450 / X65 450-600 MPa 535-760 MPa 0.93 Q/M

Elongation Af follows the API 5L equation based on specified min tensile U and test-piece area Axc. Weld-seam tensile min equals body tensile min.

CVN: mandatory for PSL2 pipe body (Table 8 at 0 °C or agreed lower T). Weld and HAZ CVN required for welded pipe. DWTT: PSL2 welded pipe per 9.9 (average shear area ≥ 85%).

Delivery Conditions for API 5L X65 PSL2

PSL2 steel-name suffixes: Q (quenched and tempered); M (thermomechanical rolled (TMCP)). Ordered as part of the steel name (e.g. X65M).

PSL2 delivery condition is part of the ordered steel name and cannot be left open. Example markings: X65N, X65Q, X65M. Plate must match the letter on the PO.

Weldability of API 5L X65 PSL2

PSL2 X65 carries mandatory CE(IIW)/Pcm limits (Table 5) that guide preheat and consumable selection. Delivery condition (Q/M) changes hardenability and HAZ response: TMCP (M) plate usually needs careful heat-input caps; Q&T (Q) plate needs HAZ toughness verification. Use low-hydrogen processes and a qualified WPS matched to the ordered steel name.

Related grades: API 5L Grade B PSL2 · API 5L X42 PSL2 · API 5L X46 PSL2 · API 5L X52 PSL2 · API 5L X56 PSL2 · API 5L X60 PSL2 · API 5L X70 PSL2 · API 5L X80 PSL2 · API 5L X65 PSL1 · API 5L X65MS

Dimensional Tolerances for API 5L X65 PSL2

Dimensional tolerances for plate follow the plate producer’s dimensional standard and the pipe mill’s order (thickness, width, flatness, edge camber). API 5L Tables 10/11 govern finished pipe OD and wall, not the plate as such. State plate tolerance class on the purchase order when nesting for LSAW.

Ultrasonic inspection of plate for laminar imperfections is commonly specified for sour (Annex H) and large-OD gas pipe; agree coverage and acceptance (e.g. related to Annex K practice) on the order.

Applications and service limits for API 5L X65 PSL2

Typical use: plate for PSL2 welded line pipe on oil and gas transmission systems that require CVN, CE control and capped Y/T. Large-OD LSAW is the main plate consumer for X65. Add Annex G when ductile-fracture arrest is specified; use MS grades for wet H2S.

  • Plate for LSAW / HFW line pipe to API 5L / ISO 3183
  • Oil and gas onshore transmission and gathering (per PSL / annex)
  • Water and utility pipelines when API 5L grade is specified
  • Bends and fittings made from matching plate when approved

Related pages: API 5L · Pipeline Steel Plates · API 5L Grade B PSL2 · API 5L X42 PSL2 · API 5L X46 PSL2 · API 5L X52 PSL2 · API 5L X56 PSL2 · API 5L X60 PSL2 · API 5L X70 PSL2 · API 5L X80 PSL2 · API 5L X65 PSL1 · API 5L X65MS

Toughness, DWTT and CE guidance for X65 PSL2

For grades > X60 to ≤ X70, full-size body CVN min average is 27 J at 0 °C for D ≤ 762 mm and 40 J for larger OD bands (Table 8). Weld/HAZ CVN min average 27 J for D < 1422 mm in grades ≤ X80.

DWTT (PSL2 welded pipe, 9.9): average shear fracture area >= 85% at 0 °C (or agreed lower temperature). For t > 25.4 mm, DWTT acceptance is by agreement. Annex G adds ductile-fracture-arrest requirements when ordered (marking suffix G).

Carbon equivalent: use CEIIW when product-analysis C > 0.12%; use CEPcm when C ≤ 0.12%. Tabulated maxima for this grade’s delivery variants are in the chemistry section (typically CEIIW 0.43 / Pcm 0.25 unless footnote says as agreed).

Y/T max 0.93 applies for D > 323.9 mm. Delivery letters allowed: Q/M.

Equivalent and related grades for API 5L X65 PSL2

These designations are commonly compared with API 5L X65 PSL2. They are approximate, not automatic substitutes. Match PSL, delivery letter, chemistry, toughness, sour testing and the project specification before replacing one grade with another.

Standard / family Grade Relation Product page
API Spec 5L (46th Edition) / ISO 3183 L450 / X65 (+ delivery letter) This page –
GB/T 21237 L450M PSL2 Approximate CN TMCP talk GB/T 21237 L450M
ISO 3183 Aligned with API 5L Same technical content family API 5L hub
Category API 5L / Pipeline hubs Navigation API 5L · Pipeline Steel Plates

API 5L X65 PSL2 vs PSL1 / related (selection aid)

Selection aid only. Not automatic substitutes.

Item X65 PSL2 X65 PSL1 X65MS
YS 450-600 MPa ≥ 450 MPa 450-600 MPa
Delivery Q/M Manufacturer option Annex H HIC
CE / CVN Mandatory Not mandatory Per page
Pages This page API 5L X65 PSL1 API 5L X65MS

Why choose SHH STEEL for API 5L X65 PSL2

  • China mill-direct supply of API 5L X65 PSL2 plate for LSAW/HFW pipe programmes
  • EN 10204 3.1 mill test certificates; 3.2 and third-party inspection (SGS, TUV, BV, ABS) on request
  • PSL, delivery letter and Annex H/G options documented on the MTC as ordered
  • Cutting, beveling and shot blasting available to shorten pipe-mill preparation
  • Family coverage: API 5L hub · Pipeline Steel Plates
  • Related planned CN plate track: GB/T 21237 pages under the pipeline plan

Supply, cutting and inspection for API 5L X65 PSL2

Item SHH STEEL supply note
Thickness Typical plate for pipe mills about 6-40 mm; thicker by mill inquiry; confirm on PO
Size Width/length per mill and nesting; cut-to-size on request
Delivery condition Q/M as ordered in steel name
Processing Cutting, beveling, shot blasting available
Mill certificate EN 10204 3.1 standard; 3.2 on request
Third-party inspection SGS, TUV, BV or ABS can be arranged
Quotation needs Grade (L450 / X65 (+ delivery letter)), PSL, delivery letter, thickness × width × length, quantity, CVN/DWTT temperature, Annex H/G if any, inspection level

FAQ

What delivery letters are allowed for X65 PSL2?
Q/M. The letter is part of the steel name on the order and MTC.
What is the Y/T limit?
Max 0.93 for D > 323.9 mm (Table 7).
Are CVN and DWTT required?
CVN is mandatory for PSL2 (Table 8). DWTT applies to PSL2 welded pipe per clause 9.9 (shear area ≥ 85%). Temperatures default to 0 °C unless a lower temperature is agreed.
When do I need X65MS?
For wet H2S / sour service see API 5L X65MS.
Is ISO 3183 identical?
It is the aligned international standard. Cite the ordered edition on the PO/MTC.

Request a quotation

Send API 5L X65 PSL2 (include delivery letter / Annex H needs), thickness × width × length, quantity, CVN/DWTT temperature, UT level and any inspection requirement. Mill availability, certification scope and a quotation will be returned.

Contact: admin@steelspecs.com · +86-18939509537 · +86-021-62716097

More options: API 5L · Pipeline Steel Plates · API 5L Grade B PSL2 · API 5L X42 PSL2 · API 5L X46 PSL2 · API 5L X52 PSL2 · API 5L X56 PSL2 · API 5L X60 PSL2 · API 5L X70 PSL2 · API 5L X80 PSL2 · API 5L X65 PSL1 · API 5L X65MS

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X