AMS 4911 Ti-6Al-4V Titanium Plate | Annealed Grade 5 (UNS R56400)

AMS 4911 Ti-6Al-4V titanium plate is annealed Grade 5 (UNS R56400 (composition similar)) supplied annealed. It is specified for 893 MPa minimum tensile strength, 827 MPa yield and 10% minimum elongation. Typical uses include airframe structural parts and fittings. SHH STEEL reviews size, finish and certificate requirements before quoting.
Keywords
AMS 4911 Ti-6Al-4V titanium plate, AMS 4911 titanium plate, UNS R56400 (composition similar) plate, annealed Grade 5 plate, AMS 4911 titanium sheet
Equivalent Grades:
UNS R56400, ASTM B265 Gr.5, ASME SB-265 Gr.5, JIS Class 60 (TAP6400), GB/T TC4, GOST VT6 (approx.), 3.7165
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is AMS 4911 Ti-6Al-4V titanium plate?

AMS 4911 Ti-6Al-4V titanium plate is made to AMS 4911, the SAE aerospace material specification for annealed Ti-6Al-4V sheet, strip and plate. It carries the UNS number R56400 (composition similar). AMS 4911 covers Ti-6Al-4V sheet, strip and plate up to 4.000 in (101.60 mm) thick in the annealed condition, with composition similar to UNS R56400. It is the standard aerospace purchasing specification for Grade 5-type flat products.

This is an alpha-beta titanium alloy. Aluminium strengthens the alpha phase and vanadium or molybdenum stabilises the beta phase, so the structure and properties depend on hot working and heat treatment. Plate is normally supplied mill annealed, giving high strength, good fatigue performance and a strength-to-weight ratio well above that of steels.

Its typical density of about 4.43 g/cm³ is a little over half that of carbon steel, which is one reason titanium plate is chosen where weight matters.

AMS specifications are written for aerospace procurement. Each covers one alloy, form and condition, and the purchaser’s drawing names the revision. Material ordered to AMS 4911 is usually bought by aerospace prime contractors and their suppliers under approved-source controls.

SHH STEEL handles Ti-6Al-4V plate enquiries within its range of titanium alloy plates and sheets, checking the ordered AMS 4911 edition, product form and certificate type before confirming supply. Related designations covered on this site include ASTM B265 Grade 5, ASME SB-265 Grade 5, JIS H4600 Class 60 TAP6400.

Material specification for AMS 4911 Ti-6Al-4V

AMS 4911 is an SAE aerospace material specification for one alloy, form and condition: Ti-6Al-4V sheet, strip and plate, annealed, up to and including 4.000 in (101.60 mm) thick. It goes beyond the industrial ASTM B265 requirements with controls on melting, microstructure and surface contamination.

Ordering item AMS 4911 basis
Specification AMS 4911, current revision unless the drawing names another
Alloy Ti-6Al-4V, composition similar to UNS R56400
Product forms Sheet, strip and plate up to 4.000 in (101.60 mm) inclusive
Melting Multiple melted; final melt by vacuum arc remelting (VAR); cold-hearth first melt permitted
Condition Sheet and strip hot rolled with or without cold reduction, annealed, descaled and levelled; plate hot rolled, annealed, descaled and flattened
Annealing 1300–1650 °F (704–899 °C), held and cooled to meet the property requirements
Quality Plate 0.500 in (12.70 mm) and over ultrasonically inspected to AMS 2631, Class A1

Plate must be produced as plate; bar, billet, forgings or forging billet may not be supplied in its place. Product must be free of alpha case and other surface contamination, checked by bend test, metallography or surface hardness. Procurement and distribution must comply with AS6279, so traceability back to the producing mill is part of the order.

Chemical composition of AMS 4911 Ti-6Al-4V (UNS R56400 (composition similar))

Composition is determined by the analytical methods required by the specification, with hydrogen determined on the product.

Element Limit, % by weight
Aluminium (Al) 5.50–6.75
Vanadium (V) 3.50–4.50
Iron (Fe) 0.30 max
Oxygen (O) 0.20 max
Carbon (C) 0.08 max
Nitrogen (N) 0.05 max (500 ppm)
Hydrogen (H) 0.015 max (150 ppm)
Yttrium (Y) 0.005 max (50 ppm)
Other elements, each 0.10 max
Other elements, total 0.40 max
Titanium (Ti) Remainder

Oxygen at 0.20% maximum is the key difference from ELI material, which is ordered to a separate specification with lower oxygen. Check analysis variations apply to product samples, not to the heat analysis reported on the certificate.

Mechanical properties of AMS 4911 Ti-6Al-4V

The values below are the requirements for Ti-6Al-4V plate in the annealed condition.

Nominal thickness, in (mm) Tensile strength, min, ksi (MPa) Yield strength 0.2% offset, min, ksi (MPa) Elongation in 2 in or 4D, min, %
Up to 0.008 (0.20), excl 134 (920) 126 (869) —
0.008–0.025 (0.20–0.63), excl 134 (920) 126 (869) 6
0.025–0.063 (0.63–1.60), excl 134 (920) 126 (869) 8
0.063–0.1875 (1.60–4.76), excl 134 (920) 126 (869) 10
0.1875–4.000 (4.76–101.60), incl 130 (893) 120 (827) 10

Bend test requirements apply to sheet and strip, with bend factors of 4.5 for product under 0.070 in (1.78 mm) and 5 for 0.070 to 0.1875 in. Microstructure must be the product of alpha-beta processing, and plate is checked for alpha case. Properties apply in the longitudinal and transverse directions as defined by the specification.

Elevated-temperature and fatigue design values are not set by the specification and come from the purchaser’s design data.

Delivery condition, finish and marking

Plate is hot rolled, annealed, descaled and flattened, with a surface comparable to a No. 1 finish on corrosion-resistant steel. Sheet and strip are hot rolled with or without cold reduction, annealed, descaled and levelled, with a surface comparable to a No. 2D finish.

  • Condition: annealed, per the specification
  • Surface: descaled, free of alpha case and other surface contamination
  • Quality: uniform, sound and free from oil cans beyond flatness tolerance, ripples and foreign material
  • Marking and packing: per the specification and the purchase order, with heat and lot identification

Report and marking requirements follow the specification revision on the order. If a size outside the specification range is ordered, the exception must be authorised by the purchaser and reported.

Welding and fabrication of Ti-6Al-4V titanium plate

Ti-6Al-4V can be welded by gas tungsten arc, plasma arc, electron beam and laser processes, but it needs more control than CP titanium.

  • Shield the weld, heat-affected zone and root with inert gas until below about 400 °C
  • Use qualified procedures and matching or engineer-approved filler metal
  • Expect lower weld-zone ductility than in the base plate; stress relief after welding is common
  • Clean joints thoroughly and avoid iron contamination

Cold formability is limited. Most forming of alpha-beta plate is done hot or by creep forming, and machining needs sharp tools, rigid set-ups and generous coolant.

Plan machining around the low thermal conductivity of the alloy: heat stays at the tool edge, so cutting speeds are low and coolant flow is high. Avoid interrupted light cuts that work-harden the surface, and keep fine chips away from ignition sources.

These are general practices, not a qualified procedure. The fabricator must qualify the welding procedure, filler metal and inspection to the applicable code.

Dimensional tolerances and flatness

Tolerances conform to AMS 2242, the SAE tolerance specification for titanium and titanium alloy sheet, strip and plate. For AMS 4911 plate, special flatness may be specified, in which case the special flatness tolerances of AMS 2242 apply.

State nominal thickness, width, length and quantity, and any cut-to-size drawing or special flatness requirement on the order. No stock sizes are implied by this page.

Titanium plate can be cut by waterjet, abrasive saw, plasma or machining. Thermal cutting leaves an oxygen-enriched edge that should be removed by machining or grinding before welding or forming, so agree the cut-edge condition and any machining allowance on the order.

Applications and service limits of Ti-6Al-4V titanium plate

Typical uses of Ti-6Al-4V plate include:

  • Airframe structural parts and fittings
  • Engine and nacelle parts up to about 750 °F (399 °C)
  • Machined aerospace components from plate
  • Ground-support and defence parts to aerospace drawings

Certain processing and service conditions may cause stress-corrosion cracking; the specification refers users to ARP982. Alpha-beta alloys resist seawater and many oxidizing media well, but they are less resistant than CP titanium in hot reducing acids. They are not suited to hydrofluoric acid, fluoride-bearing media, dry chlorine or red fuming nitric acid. Maximum service temperature and fatigue design values come from the applicable design code, not from the plate specification.

When selecting Ti-6Al-4V, compare it with ASTM B265 Grade 5, ASME SB-265 Grade 5, JIS H4600 Class 60 (TAP6400). The choice usually turns on the balance of strength, formability, corrosion behaviour in the actual medium and cost, and on which standard the drawing or design code names.

Compare Ti-6Al-4V with related grades

The grades below are commonly compared with this material across standards. Values are minimum tensile, yield and minimum elongation as set by each standard.

Grade Tensile strength Yield / proof strength Elongation, min Typical role
Ti-6Al-4V, annealed 130 ksi (893 MPa) 120 ksi (827 MPa) min 10% Aerospace Ti-6Al-4V annealed plate
ASTM B265 Grade 5 (R56400) 130 ksi (895 MPa) 120 ksi (828 MPa) min 10% Workhorse alpha-beta alloy
ASME SB-265 Grade 5 (R56400) 130 ksi (895 MPa) 120 ksi (828 MPa) min 10% Workhorse alpha-beta alloy
JIS H4600 Class 60 (TAP6400) 895 MPa min 825 MPa min 10% Ti-6Al-4V, high strength
GB/T 3621 TC4 895 MPa min 830 MPa min 12% Ti-6Al-4V alpha-beta

A higher strength level is not automatically better. Interstitial limits, toughness, bend radius and fatigue behaviour differ between grades, so changes need engineer approval.

AMS 4911 Ti-6Al-4V equivalent grades

The designations below are commonly compared with AMS 4911 Ti-6Al-4V. They are close in composition and role, but limits, tests and product forms are set by each standard, so they are not automatically interchangeable.

Standard / system Designation Relationship to AMS 4911 Ti-6Al-4V
ASTM B265 Grade 5 Close equivalent; ASTM limits and tests apply
ASME SB-265 Grade 5 ASME Code version of the ASTM grade; ordered for pressure equipment
JIS H4600 Class 60 (TAP6400) Close equivalent; JIS strength range and tests differ
GB/T 3621 TC4 Close equivalent; confirm grade name and limits in the ordered edition
GOST 22178 VT6 Approximate; GOST limits and sheet scope differ
UNS R56400 Same unified number as ASTM Grade 5
DIN / EN material number 3.7165 (TiAl6V4) Close equivalent; aerospace EN specifications add their own tests

Where a drawing names one designation and the supplier offers another, agree in writing which standard governs chemistry, tensile values, testing and marking. Dual or multiple certification is possible only when the material meets every cited standard in full, and the certificate must show the results against each one.

Why choose SHH STEEL for Ti-6Al-4V titanium plate

SHH STEEL supports specification-led purchasing of titanium plate and sheet.

  • We quote to the AMS 4911 revision on your drawing and check melting route, ultrasonic class and traceability
  • Certificates are checked against the composition, tensile, bend and microstructure requirements
  • Sizes, quantities, testing and delivery are confirmed in the quotation, not assumed
  • Finish, marking and packing are agreed before production

Questions on equivalents, dual certification or edition changes are answered before an order is placed.

How to enquire for AMS 4911 Ti-6Al-4V plate

Send the material schedule with the details below. We review the enquiry and raise any open points before confirming the supply route.

Enquiry item Information required
Material AMS 4911 Ti-6Al-4V annealed, revision
Product form Plate, sheet or strip; for sheet, cold or hot rolled
Dimensions Thickness, width, length, quantity and any cutting drawing
Finish Descaled, sandblasted, ground or other agreed surface
Testing Ultrasonic class for plate 0.500 in and over, any extra tests
Documents Certificate type and any third-party inspection
Destination Delivery place and packing requirements

FAQ

Is AMS 4911 the same as ASTM B265 Grade 5?
Both cover Ti-6Al-4V with composition similar to UNS R56400, but AMS 4911 adds aerospace requirements such as VAR final melting, microstructure limits, alpha-case checks and ultrasonic testing of thicker plate. B265 Grade 5 plate does not automatically meet AMS 4911.
What is the tensile strength of AMS 4911 Ti-6Al-4V titanium plate?
The requirement is 130 ksi (893 MPa) minimum for plate over 0.1875 in. The 0.2% proof or yield strength is 120 ksi (827 MPa) minimum for plate. Minimum elongation is 10%. Values apply to the condition and thickness range stated in the standard.
What is Ti-6Al-4V mainly used for?
Typical uses include airframe structural parts and fittings, engine and nacelle parts up to about 750 °F (399 °C) and machined aerospace components from plate. Certain processing and service conditions may cause stress-corrosion cracking; the specification refers users to ARP982.
What thickness does AMS 4911 cover?
Sheet, strip and plate up to and including 4.000 in (101.60 mm). Plate 0.500 in (12.70 mm) and over is ultrasonically inspected to AMS 2631 Class A1.
What should I send for a quotation?
Send AMS 4911 Ti-6Al-4V, the edition, product form, thickness, width, length and quantity, the finish, any special testing, the certificate type and the destination.

Request a quotation for AMS 4911 Ti-6Al-4V titanium plate

AMS 4911 Ti-6Al-4V is annealed Grade 5, UNS R56400 (composition similar), specified for 130 ksi (893 MPa) minimum for plate over 0.1875 in tensile strength, 120 ksi (827 MPa) minimum for plate yield or proof strength and 10% minimum elongation in the annealed condition. Typical uses include airframe structural parts and fittings and engine and nacelle parts up to about 750 °F (399 °C).

Send the product form, sizes, quantity, finish, certificate type and destination to SHH STEEL. Compare other grades on the AMS 4911 page or browse all titanium alloy plates and sheets. Availability, testing and delivery are confirmed against each enquiry.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X