SA-500 Grade B Steel Hollow Sections (ASTM A500/A500M Basis) | SA-500 Steel Hollow Sections - SHH STEEL

SA-500 Grade B Steel Hollow Sections (ASTM A500/A500M Basis)

Enquiries named SA-500 for Grade B HSS are described here on the technical basis of ASTM A500/A500M-23. Grade B requires 58 ksi [400 MPa] tensile strength and 46 ksi [315 MPa] yield. This page does not treat SA-500 as a listed BPVC specification. Typographical sizes follow the AISC 15th Edition HSS subset on the ASTM A500 Grade B page.
Keywords
SA-500 Grade B HSS, SA-500 Grade B hollow section, ASTM A500/A500M basis, SA-500 steel tubing enquiry, A500 Grade B companion
Equivalent Grades:
Near-equivalents only, not automatic substitutes.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Size Chart
Applications
Comparison
Equivalent Grades
Sourcing
FAQ
Conclusion

What Does an SA-500 Grade B HSS Enquiry Mean?

Purchase enquiries sometimes name SA-500, or SA-500M, for Grade B cold-formed hollow structural sections. The chemistry and mechanical values on this page are those of ASTM A500/A500M-23 Grade B. The edition named on the purchase order governs delivery.

This page does not replace ASTM A500 Grade B Steel Hollow Sections (HSS). That product remains the ASTM A500 Grade B page. The two documents should be read together when an enquiry uses the SA-500 name for Grade B HSS. An ASTM A500 certificate is not automatically an SA-500 document.

Technical Basis for SA-500 Grade B Enquiries: ASTM A500/A500M-23, Not a Cited BPVC Listing

ASTM A500/A500M-23 covers cold-formed welded and seamless carbon steel round, square, rectangular, or special-shape structural tubing. Grade B is the grade named on this page. Table 2 of that edition gives Grade B a single 58 ksi [400 MPa] tensile minimum and a single 46 ksi [315 MPa] yield minimum for all shapes.

The ASME BPVC Section II, Part A specification lists reviewed for this site for the 2023 and 2025 editions do not contain an SA-500 or SA-500M entry in the record used here. This page therefore does not assign an identical-with year, does not treat SA-500 as a listed Code specification, and does not apply an ASME mark to the product. A later Code addendum can change that record; the lists actually reviewed remain the ones named above. The existing SA-992 companion on this site uses the same “basis, not a cited listing” treatment.

Hot-formed ASTM A501 Grade B tubing is a different specification with a different yield table. It is not the basis of this companion.

Chemical Composition for SA-500 Grade B Enquiries (ASTM A500/A500M-23 Basis)

The table recites the ASTM A500/A500M-23 Table 1 Grade B (and D) limits used on the live Grade B page. This companion is Grade B only. Grade C has its own chemistry and mechanical row and is not this product.

Swipe horizontally to view all dimensions.

Element Grade B heat analysis Grade B product analysis Notes
C, max (%) 0.26 0.30 A500/A500M-23 Table 1 for Grades B and D; this page is Grade B.
Mn, max (%) 1.35 1.40 A footnote in Table 1 permits a higher manganese maximum, to 1.50 % heat and 1.60 % product, with the associated carbon adjustment.
P, max (%) 0.035 0.045 —
S, max (%) 0.035 0.045 —
Cu, min (%), when copper steel is specified 0.20 0.18 Applies only when copper steel is specified on the order.

Mechanical Properties for SA-500 Grade B Enquiries (ASTM A500/A500M-23 Basis)

Grade B requires 58 ksi [400 MPa] minimum tensile strength and 46 ksi [315 MPa] minimum yield strength for all shapes. Elongation is 23 % in 2 in. [50 mm] when the specified wall is at least 0.180 in. [4.57 mm]; thinner walls use the Table 2 formula 61 t + 12. Do not replace this row with the A501 Grade B yield-by-wall table.

Swipe horizontally to view all dimensions.

Property Requirement for Grade B, all shapes (A500/A500M-23 Table 2)
Tensile strength, min 58 ksi [400 MPa]
Yield strength, min 46 ksi [315 MPa]
Elongation in 2 in. [50 mm], min, for specified wall ≥ 0.180 in. [4.57 mm] 23 %
Elongation, thinner walls The Table 2 formula 61 t + 12 applies when the specified wall is below 0.180 in. [4.57 mm]; a single 23 % figure is not used in that band.

SA-500 Grade B Enquiry Sizes: AISC Manual 15th Edition HSS (ASTM A500 Basis)

Enquiries named SA-500 for Grade B HSS use the same 516 hollow structural section designations from the AISC Steel Construction Manual, 15th Edition, shape file (Type = HSS) as ASTM A500 Grade B Steel Hollow Sections (HSS), because the technical basis on this companion is ASTM A500/A500M-23: 107 square, 281 rectangular and 128 round. Each row joins the inch-pound and SI companion records already used for the live A36 W-shape and S-shape tables. They are reference dimensions for identification and estimating, not a rolling list, and not a claim that every HSS designation is produced, or is currently available, in Grade B, and not a listed ASME BPVC size table. A500/A500M-23 limits the periphery to 88 in [2235 mm] and the specified wall thickness to 1.000 in [25.4 mm]; every listed designation lies inside those limits (the largest square, HSS 22×22, has a 88 in periphery).

A designation such as HSS 8×8×½ or HSS 20.000×0.375 is a size call: outside dimensions and a specified (nominal) wall. The file also publishes a design wall thickness, tdes, which is about 0.93 of the nominal wall on these rows — the usual AISC practice for electric-resistance-welded A500 HSS. Use the specified wall when ordering and the design wall when the design specification requires it; do not treat the two as interchangeable on the certificate. Corner radii are omitted because a single delivery radius is not published as a unique column in this file, and a radius is not invented here.

Theoretical mass is the tabulated reference value. Settlement should follow the contract — tabulated theoretical mass or weighed mass — and the dimensional tolerances of the ordered A500/A500M edition (not ASTM A6/A6M, which applies to rolled shapes, not to this tubing). These HSS rows are not interchangeable with AISC Pipe designations, with ASTM A53 pipe, or with EN 10219, EN 10210 or GB/T 6728 hollow sections of a similar outside size.

Square HSS (SHS)

107 square designations, grouped by outside size. The first group is the larger squares, from HSS 22×22 down through HSS 10×10.

HSS 22×22 to HSS 10×10

36 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation B (in) B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 22×22×7/8 HSS 558.8×558.8×22.2 22 559 0.875 22.2 0.814 20.7 67.3 43400 244.88 364
HSS 22×22×3/4 HSS 558.8×558.8×19 22 559 0.75 19.1 0.698 17.7 58.2 37600 212 315
HSS 20×20×7/8 HSS 508×508×22.2 20 508 0.875 22.2 0.814 20.7 60.8 39200 221.06 329
HSS 20×20×3/4 HSS 508×508×19 20 508 0.75 19.1 0.698 17.7 52.6 33900 191.58 285
HSS 20×20×5/8 HSS 508×508×15.9 20 508 0.625 15.9 0.581 14.8 44.3 28600 161.4 240
HSS 20×20×1/2 HSS 508×508×12.7 20 508 0.5 12.7 0.465 11.8 35.8 23100 130.52 194
HSS 18×18×7/8 HSS 457.2×457.2×22.2 18 457 0.875 22.2 0.814 20.7 54.3 35000 197.24 293
HSS 18×18×3/4 HSS 457.2×457.2×19 18 457 0.75 19.1 0.698 17.7 47.1 30400 171.16 255
HSS 18×18×5/8 HSS 457.2×457.2×15.9 18 457 0.625 15.9 0.581 14.8 39.6 25500 144.39 215
HSS 18×18×1/2 HSS 457.2×457.2×12.7 18 457 0.5 12.7 0.465 11.8 32.1 20700 116.91 174
HSS 16×16×7/8 HSS 406.4×406.4×22.2 16 406 0.875 22.2 0.814 20.7 47.7 30800 173.43 258
HSS 16×16×3/4 HSS 406.4×406.4×19.0 16 406 0.75 19.1 0.698 17.7 41.5 26800 150.75 224
HSS 16×16×5/8 HSS 406.4×406.4×15.9 16 406 0.625 15.9 0.581 14.8 35 22600 127.37 189
HSS 16×16×1/2 HSS 406.4×406.4×12.7 16 406 0.5 12.7 0.465 11.8 28.3 18300 103.3 153
HSS 16×16×3/8 HSS 406.4×406.4×9.5 16 406 0.375 9.53 0.349 8.86 21.5 13900 78.52 117
HSS 16×16×5/16 HSS 406.4×406.4×7.9 16 406 0.3125 7.94 0.291 7.39 18.1 11700 65.87 97.9
HSS 14×14×7/8 HSS 355.6×355.6×22.2 14 356 0.875 22.2 0.814 20.7 41.2 26600 149.61 223
HSS 14×14×3/4 HSS 355.6×355.6×19 14 356 0.75 19.1 0.698 17.7 35.9 23200 130.33 194
HSS 14×14×5/8 HSS 355.6×355.6×15.9 14 356 0.625 15.9 0.581 14.8 30.3 19500 110.36 164
HSS 14×14×1/2 HSS 355.6×355.6×12.7 14 356 0.5 12.7 0.465 11.8 24.6 15900 89.68 133
HSS 14×14×3/8 HSS 355.6×355.6×9.5 14 356 0.375 9.53 0.349 8.86 18.7 12100 68.31 102
HSS 14×14×5/16 HSS 355.6×355.6×7.9 14 356 0.3125 7.94 0.291 7.39 15.7 10100 57.36 85.3
HSS 12×12×3/4 HSS 304.8×304.8×19 12 305 0.75 19.1 0.698 17.7 30.3 19500 109.91 164
HSS 12×12×5/8 HSS 304.8×304.8×15.9 12 305 0.625 15.9 0.581 14.8 25.7 16600 93.34 139
HSS 12×12×1/2 HSS 304.8×304.8×12.7 12 305 0.5 12.7 0.465 11.8 20.9 13500 76.07 113
HSS 12×12×3/8 HSS 304.8×304.8×9.5 12 305 0.375 9.53 0.349 8.86 16 10300 58.1 86.3
HSS 12×12×5/16 HSS 304.8×304.8×7.9 12 305 0.3125 7.94 0.291 7.39 13.4 8650 48.86 72.6
HSS 12×12×1/4 HSS 304.8×304.8×6.4 12 305 0.25 6.35 0.233 5.92 10.8 6970 39.43 58.6
HSS 12×12×3/16 HSS 304.8×304.8×4.8 12 305 0.1875 4.76 0.174 4.42 8.15 5260 29.84 44.4
HSS 10×10×3/4 HSS 254×254×19 10 254 0.75 19.1 0.698 17.7 24.7 15900 89.5 133
HSS 10×10×5/8 HSS 254×254×15.9 10 254 0.625 15.9 0.581 14.8 21 13500 76.33 113
HSS 10×10×1/2 HSS 254×254×12.7 10 254 0.5 12.7 0.465 11.8 17.2 11100 62.46 92.7
HSS 10×10×3/8 HSS 254×254×9.5 10 254 0.375 9.53 0.349 8.86 13.2 8520 47.9 71.2
HSS 10×10×5/16 HSS 254×254×7.9 10 254 0.3125 7.94 0.291 7.39 11.1 7160 40.35 60
HSS 10×10×1/4 HSS 254×254×6.4 10 254 0.25 6.35 0.233 5.92 8.96 5780 32.63 48.5
HSS 10×10×3/16 HSS 254×254×4.8 10 254 0.1875 4.76 0.174 4.42 6.76 4360 24.73 36.8

HSS 9×9 to HSS 6×6

28 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation B (in) B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 9×9×5/8 HSS 228.6×228.6×15.9 9 229 0.625 15.9 0.581 14.8 18.7 12100 67.82 101
HSS 9×9×1/2 HSS 228.6×228.6×12.7 9 229 0.5 12.7 0.465 11.8 15.3 9870 55.66 82.6
HSS 9×9×3/8 HSS 228.6×228.6×9.5 9 229 0.375 9.53 0.349 8.86 11.8 7610 42.79 63.6
HSS 9×9×5/16 HSS 228.6×228.6×7.9 9 229 0.3125 7.94 0.291 7.39 9.92 6400 36.1 53.6
HSS 9×9×1/4 HSS 228.6×228.6×6.4 9 229 0.25 6.35 0.233 5.92 8.03 5180 29.23 43.4
HSS 9×9×3/16 HSS 228.6×228.6×74.8 9 229 0.1875 4.76 0.174 4.42 6.06 3910 22.18 33
HSS 9×9×1/8 HSS 228.6×228.6×3.2 9 229 0.125 3.18 0.116 2.95 4.09 2640 14.96 22.3
HSS 8×8×5/8 HSS 203.2×203.2×15.9 8 203 0.625 15.9 0.581 14.8 16.4 10600 59.32 88
HSS 8×8×1/2 HSS 203.2×203.2×12.7 8 203 0.5 12.7 0.465 11.8 13.5 8710 48.85 72.5
HSS 8×8×3/8 HSS 203.2×203.2×9.5 8 203 0.375 9.53 0.349 8.86 10.4 6710 37.69 56
HSS 8×8×5/16 HSS 203.2×203.2×7.9 8 203 0.3125 7.94 0.291 7.39 8.76 5650 31.84 47.3
HSS 8×8×1/4 HSS 203.2×203.2×6.4 8 203 0.25 6.35 0.233 5.92 7.1 4580 25.82 38.4
HSS 8×8×3/16 HSS 203.2×203.2×4.8 8 203 0.1875 4.76 0.174 4.42 5.37 3460 19.63 29.2
HSS 8×8×1/8 HSS 203.2×203.2×3.2 8 203 0.125 3.18 0.116 2.95 3.62 2340 13.26 19.7
HSS 7×7×5/8 HSS 177.8×177.8×15.9 7 178 0.625 15.9 0.581 14.8 14 9030 50.81 75.3
HSS 7×7×1/2 HSS 177.8×177.8×12.7 7 178 0.5 12.7 0.465 11.8 11.6 7480 42.05 62.4
HSS 7×7×3/8 HSS 177.8×177.8×9.5 7 178 0.375 9.53 0.349 8.86 8.97 5790 32.58 48.4
HSS 7×7×5/16 HSS 177.8×177.8×7.9 7 178 0.3125 7.94 0.291 7.39 7.59 4900 27.59 41
HSS 7×7×1/4 HSS 177.8×177.8×6.4 7 178 0.25 6.35 0.233 5.92 6.17 3980 22.42 33.3
HSS 7×7×3/16 HSS 177.8×177.8×4.8 7 178 0.1875 4.76 0.174 4.42 4.67 3010 17.08 25.4
HSS 7×7×1/8 HSS 177.8×177.8×3.2 7 178 0.125 3.18 0.116 2.95 3.16 2040 11.56 17.2
HSS 6×6×5/8 HSS 152.4×152.4×15.9 6 152 0.625 15.9 0.581 14.8 11.7 7550 42.3 62.6
HSS 6×6×1/2 HSS 152.4×152.4×12.7 6 152 0.5 12.7 0.465 11.8 9.74 6280 35.24 52.2
HSS 6×6×3/8 HSS 152.4×152.4×9.5 6 152 0.375 9.53 0.349 8.86 7.58 4890 27.48 40.8
HSS 6×6×5/16 HSS 152.4×152.4×7.9 6 152 0.3125 7.94 0.291 7.39 6.43 4150 23.34 34.6
HSS 6×6×1/4 HSS 152.4×152.4×6.4 6 152 0.25 6.35 0.233 5.92 5.24 3380 19.02 28.3
HSS 6×6×3/16 HSS 152.4×152.4×4.8 6 152 0.1875 4.76 0.174 4.42 3.98 2570 14.53 21.6
HSS 6×6×1/8 HSS 152.4×152.4×3.2 6 152 0.125 3.18 0.116 2.95 2.7 1740 9.86 14.7

HSS 5.5×5.5 to HSS 2×2

43 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation B (in) B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 5-1/2×5-1/2×3/8 HSS 139.7×139.7×9.5 5.5 140 0.375 9.53 0.349 8.86 6.88 4440 24.93 37
HSS 5-1/2×5-1/2×5/16 HSS 139.7×139.7×7.9 5.5 140 0.3125 7.94 0.291 7.39 5.85 3770 21.21 31.5
HSS 5-1/2×5-1/2×1/4 HSS 139.7×139.7×6.4 5.5 140 0.25 6.35 0.233 5.92 4.77 3080 17.32 25.7
HSS 5-1/2×5-1/2×3/16 HSS 139.7×139.7×4.8 5.5 140 0.1875 4.76 0.174 4.42 3.63 2340 13.25 19.7
HSS 5-1/2×5-1/2×1/8 HSS 139.7×139.7×3.2 5.5 140 0.125 3.18 0.116 2.95 2.46 1590 9.01 13.4
HSS 5×5×1/2 HSS 127×127×12.7 5 127 0.5 12.7 0.465 11.8 7.88 5080 28.43 42.1
HSS 5×5×3/8 HSS 127×127×9.5 5 127 0.375 9.53 0.349 8.86 6.18 3990 22.37 33.2
HSS 5×5×5/16 HSS 127×127×7.9 5 127 0.3125 7.94 0.291 7.39 5.26 3390 19.08 28.3
HSS 5×5×1/4 HSS 127×127×6.4 5 127 0.25 6.35 0.233 5.92 4.3 2770 15.62 23.2
HSS 5×5×3/16 HSS 127×127×4.8 5 127 0.1875 4.76 0.174 4.42 3.28 2120 11.97 17.8
HSS 5×5×1/8 HSS 127×127×3.2 5 127 0.125 3.18 0.116 2.95 2.23 1440 8.16 12.1
HSS 4-1/2×4-1/2×1/2 HSS 114.3×114.3×12.7 4.5 114 0.5 12.7 0.465 11.8 6.95 4480 25.03 37.1
HSS 4-1/2×4-1/2×3/8 HSS 114.3×114.3×9.5 4.5 114 0.375 9.53 0.349 8.86 5.48 3540 19.82 29.4
HSS 4-1/2×4-1/2×5/16 HSS 114.3×114.3×7.9 4.5 114 0.3125 7.94 0.291 7.39 4.68 3020 16.96 25.2
HSS 4-1/2×4-1/2×1/4 HSS 114.3×114.3×6.4 4.5 114 0.25 6.35 0.233 5.92 3.84 2480 13.91 20.7
HSS 4-1/2×4-1/2×3/16 HSS 114.3×114.3×4.8 4.5 114 0.1875 4.76 0.174 4.42 2.93 1890 10.7 15.9
HSS 4-1/2×4-1/2×1/8 HSS 114.3×114.3×3.2 4.5 114 0.125 3.18 0.116 2.95 2 1290 7.31 10.9
HSS 4×4×1/2 HSS 101.6×101.6×12.7 4 102 0.5 12.7 0.465 11.8 6.02 3880 21.63 32
HSS 4×4×3/8 HSS 101.6×101.6×9.5 4 102 0.375 9.53 0.349 8.86 4.78 3080 17.27 25.6
HSS 4×4×5/16 HSS 101.6×101.6×7.9 4 102 0.3125 7.94 0.291 7.39 4.1 2650 14.83 22
HSS 4×4×1/4 HSS 101.6×101.6×6.4 4 102 0.25 6.35 0.233 5.92 3.37 2170 12.21 18.1
HSS 4×4×3/16 HSS 101.6×101.6×4.8 4 102 0.1875 4.76 0.174 4.42 2.58 1660 9.42 14
HSS 4×4×1/8 HSS 101.6×101.6×3.2 4 102 0.125 3.18 0.116 2.95 1.77 1140 6.46 9.59
HSS 3-1/2×3-1/2×3/8 HSS 88.9×88.9×9.5 3.5 88.9 0.375 9.53 0.349 8.86 4.09 2640 14.72 21.8
HSS 3-1/2×3-1/2×5/16 HSS 88.9×88.9×7.9 3.5 88.9 0.3125 7.94 0.291 7.39 3.52 2270 12.7 18.8
HSS 3-1/2×3-1/2×1/4 HSS 88.9×88.9×6.4 3.5 88.9 0.25 6.35 0.233 5.92 2.91 1880 10.51 15.6
HSS 3-1/2×3-1/2×3/16 HSS 88.9×88.9×4.8 3.5 88.9 0.1875 4.76 0.174 4.42 2.24 1450 8.15 12.1
HSS 3-1/2×3-1/2×1/8 HSS 88.9×88.9×3.2 3.5 88.9 0.125 3.18 0.116 2.95 1.54 994 5.61 8.33
HSS 3×3×3/8 HSS 76.2×76.2×9.5 3 76.2 0.375 9.53 0.349 8.86 3.39 2190 12.17 18
HSS 3×3×5/16 HSS 76.2×76.2×7.9 3 76.2 0.3125 7.94 0.291 7.39 2.94 1900 10.58 15.7
HSS 3×3×1/4 HSS 76.2×76.2×6.4 3 76.2 0.25 6.35 0.233 5.92 2.44 1570 8.81 13.1
HSS 3×3×3/16 HSS 76.2×76.2×4.8 3 76.2 0.1875 4.76 0.174 4.42 1.89 1220 6.87 10.2
HSS 3×3×1/8 HSS 76.2×76.2×3.2 3 76.2 0.125 3.18 0.116 2.95 1.3 839 4.75 7.06
HSS 2-1/2×2-1/2×5/16 HSS 63.5×63.5×7.9 2.5 63.5 0.3125 7.94 0.291 7.39 2.35 1520 8.45 12.5
HSS 2-1/2×2-1/2×1/4 HSS 63.5×63.5×6.4 2.5 63.5 0.25 6.35 0.233 5.92 1.97 1270 7.11 10.5
HSS 2-1/2×2-1/2×3/16 HSS 63.5×63.5×4.8 2.5 63.5 0.1875 4.76 0.174 4.42 1.54 994 5.59 8.3
HSS 2-1/2×2-1/2×1/8 HSS 63.5×63.5×3.2 2.5 63.5 0.125 3.18 0.116 2.95 1.07 690 3.9 5.8
HSS 2-1/4×2-1/4×1/4 HSS 57.2×57.2×6.4 2.25 57.2 0.25 6.35 0.233 5.92 1.74 1120 6.26 9.26
HSS 2-1/4×2-1/4×3/16 HSS 57.2×57.2×4.8 2.25 57.2 0.1875 4.76 0.174 4.42 1.37 884 4.96 7.35
HSS 2-1/4×2-1/4×1/8 HSS 57.2×57.2×3.2 2.25 57.2 0.125 3.18 0.116 2.95 0.956 617 3.48 5.16
HSS 2×2×1/4 HSS 50.8×50.8×6.4 2 50.8 0.25 6.35 0.233 5.92 1.51 974 5.41 8
HSS 2×2×3/16 HSS 50.8×50.8×4.8 2 50.8 0.1875 4.76 0.174 4.42 1.19 768 4.32 6.4
HSS 2×2×1/8 HSS 50.8×50.8×3.2 2 50.8 0.125 3.18 0.116 2.95 0.84 542 3.05 4.53

Rectangular HSS (RHS)

281 rectangular designations, grouped by the longer outside dimension.

HSS 24×… to HSS 16×…

37 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation H×B (in) H×B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 24×12×3/4 HSS 609.6×304.8×19 24×12 610×305 0.75 19.1 0.698 17.7 47.1 30400 171.16 255
HSS 24×12×5/8 HSS 609.6×304.8×15.9 24×12 610×305 0.625 15.9 0.581 14.8 39.6 25500 144.39 215
HSS 24×12×1/2 HSS 609.6×304.8×12.7 24×12 610×305 0.5 12.7 0.465 11.8 32.1 20700 116.91 174
HSS 20×12×3/4 HSS 508×304.8×19 20×12 508×305 0.75 19.1 0.698 17.7 41.5 26800 150.75 224
HSS 20×12×5/8 HSS 508×304.8×15.9 20×12 508×305 0.625 15.9 0.581 14.8 35 22600 127.37 189
HSS 20×12×1/2 HSS 508×304.8×12.7 20×12 508×305 0.5 12.7 0.465 11.8 28.3 18300 103.3 153
HSS 20×12×3/8 HSS 508×304.8×9.5 20×12 508×305 0.375 9.53 0.349 8.86 21.5 13900 78.52 117
HSS 20×12×5/16 HSS 508×304.8×7.9 20×12 508×305 0.3125 7.94 0.291 7.39 18.1 11700 65.87 97.9
HSS 20×8×5/8 HSS 508×203.2×15.9 20×8 508×203 0.625 15.9 0.581 14.8 30.3 19500 110.36 164
HSS 20×8×1/2 HSS 508×203.2×12.7 20×8 508×203 0.5 12.7 0.465 11.8 24.6 15900 89.68 133
HSS 20×8×3/8 HSS 508×203.2×9.5 20×8 508×203 0.375 9.53 0.349 8.86 18.7 12100 68.31 102
HSS 20×8×5/16 HSS 508×203.2×7.9 20×8 508×203 0.3125 7.94 0.291 7.39 15.7 10100 57.36 85.3
HSS 20×4×1/2 HSS 508×101.6×12.7 20×4 508×102 0.5 12.7 0.465 11.8 20.9 13500 76.07 113
HSS 20×4×3/8 HSS 508×101.6×9.5 20×4 508×102 0.375 9.53 0.349 8.86 16 10300 58.1 86.4
HSS 20×4×5/16 HSS 508×101.6×7.9 20×4 508×102 0.3125 7.94 0.291 7.39 13.4 8650 48.86 72.7
HSS 20×4×1/4 HSS 508×101.6×6.4 20×4 508×102 0.25 6.35 0.233 5.92 10.8 6970 39.43 58.7
HSS 18×6×5/8 HSS 457.2×152.4×15.9 18×6 457×152 0.625 15.9 0.581 14.8 25.7 16600 93.34 139
HSS 18×6×1/2 HSS 457.2×152.4×12.7 18×6 457×152 0.5 12.7 0.465 11.8 20.9 13500 76.07 113
HSS 18×6×3/8 HSS 457.2×152.4×9.5 18×6 457×152 0.375 9.53 0.349 8.86 16 10300 58.1 86.4
HSS 18×6×5/16 HSS 457.2×152.4×7.9 18×6 457×152 0.3125 7.94 0.291 7.39 13.4 8650 48.86 72.7
HSS 18×6×1/4 HSS 457.2×152.4×6.4 18×6 457×152 0.25 6.35 0.233 5.92 10.8 6970 39.43 58.7
HSS 16×12×3/4 HSS 406.4×304.8×19 16×12 406×305 0.75 19.1 0.698 17.7 35.9 23200 130.33 194
HSS 16×12×5/8 HSS 406.4×304.8×15.9 16×12 406×305 0.625 15.9 0.581 14.8 30.3 19500 110.36 164
HSS 16×12×1/2 HSS 406.4×304.8×12.7 16×12 406×305 0.5 12.7 0.465 11.8 24.6 15900 89.68 133
HSS 16×12×3/8 HSS 406.4×304.8×9.5 16×12 406×305 0.375 9.53 0.349 8.86 18.7 12100 68.31 102
HSS 16×12×5/16 HSS 406.4×304.8×7.9 16×12 406×305 0.3125 7.94 0.291 7.39 15.7 10100 57.36 85.4
HSS 16×8×5/8 HSS 406.4×203.2×15.9 16×8 406×203 0.625 15.9 0.581 14.8 25.7 16600 93.34 139
HSS 16×8×1/2 HSS 406.4×203.2×12.7 16×8 406×203 0.5 12.7 0.465 11.8 20.9 13500 76.07 113
HSS 16×8×3/8 HSS 406.4×203.2×9.5 16×8 406×203 0.375 9.53 0.349 8.86 16 10300 58.1 86.4
HSS 16×8×5/16 HSS 406.4×203.2×7.9 16×8 406×203 0.3125 7.94 0.291 7.39 13.4 8650 48.86 72.7
HSS 16×8×1/4 HSS 406.4×203.2×6.4 16×8 406×203 0.25 6.35 0.233 5.92 10.8 6970 39.43 58.7
HSS 16×4×5/8 HSS 406.4×101.6×15.9 16×4 406×102 0.625 15.9 0.581 14.8 21 13500 76.33 113
HSS 16×4×1/2 HSS 406.4×101.6×12.7 16×4 406×102 0.5 12.7 0.465 11.8 17.2 11100 62.46 92.7
HSS 16×4×3/8 HSS 406.4×101.6×9.5 16×4 406×102 0.375 9.53 0.349 8.86 13.2 8520 47.9 71.2
HSS 16×4×5/16 HSS 406.4×101.6×7.9 16×4 406×102 0.3125 7.94 0.291 7.39 11.1 7160 40.35 60
HSS 16×4×1/4 HSS 406.4×101.6×6.4 16×4 406×102 0.25 6.35 0.233 5.92 8.96 5780 32.63 48.6
HSS 16×4×3/16 HSS 406.4×101.6×4.8 16×4 406×102 0.1875 4.76 0.174 4.42 6.76 4360 24.73 36.7

HSS 14×… to HSS 10×…

86 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation H×B (in) H×B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 14×10×5/8 HSS 355.6×254×15.9 14×10 356×254 0.625 15.9 0.581 14.8 25.7 16600 93.34 139
HSS 14×10×1/2 HSS 355.6×254×12.7 14×10 356×254 0.5 12.7 0.465 11.8 20.9 13500 76.07 113
HSS 14×10×3/8 HSS 355.6×254×9.5 14×10 356×254 0.375 9.53 0.349 8.86 16 10300 58.1 86.4
HSS 14×10×5/16 HSS 355.6×254×7.9 14×10 356×254 0.3125 7.94 0.291 7.39 13.4 8650 48.86 72.7
HSS 14×10×1/4 HSS 355.6×254×6.4 14×10 356×254 0.25 6.35 0.233 5.92 10.8 6970 39.43 58.7
HSS 14×6×5/8 HSS 355.6×152.4×15.9 14×6 356×152 0.625 15.9 0.581 14.8 21 13500 76.33 113
HSS 14×6×1/2 HSS 355.6×152.4×12.7 14×6 356×152 0.5 12.7 0.465 11.8 17.2 11100 62.46 92.7
HSS 14×6×3/8 HSS 355.6×152.4×9.5 14×6 356×152 0.375 9.53 0.349 8.86 13.2 8520 47.9 71.2
HSS 14×6×5/16 HSS 355.6×152.4×7.9 14×6 356×152 0.3125 7.94 0.291 7.39 11.1 7160 40.35 60
HSS 14×6×1/4 HSS 355.6×152.4×6.4 14×6 356×152 0.25 6.35 0.233 5.92 8.96 5780 32.63 48.6
HSS 14×6×3/16 HSS 355.6×152.4×4.8 14×6 356×152 0.1875 4.76 0.174 4.42 6.76 4360 24.73 36.7
HSS 14×4×5/8 HSS 355.6×101.6×15.9 14×4 356×102 0.625 15.9 0.581 14.8 18.7 12100 67.82 101
HSS 14×4×1/2 HSS 355.6×101.6×12.7 14×4 356×102 0.5 12.7 0.465 11.8 15.3 9870 55.66 82.6
HSS 14×4×3/8 HSS 355.6×101.6×9.5 14×4 356×102 0.375 9.53 0.349 8.86 11.8 7610 42.79 63.6
HSS 14×4×5/16 HSS 355.6×101.6×7.9 14×4 356×102 0.3125 7.94 0.291 7.39 9.92 6400 36.1 53.7
HSS 14×4×1/4 HSS 355.6×101.6×6.4 14×4 356×102 0.25 6.35 0.233 5.92 8.03 5180 29.23 43.5
HSS 14×4×3/16 HSS 355.6×101.6×4.8 14×4 356×102 0.1875 4.76 0.174 4.42 6.06 3910 22.18 32.9
HSS 12×10×1/2 HSS 304.8×254×12.7 12×10 305×254 0.5 12.7 0.465 11.8 19 12300 69.27 103
HSS 12×10×3/8 HSS 304.8×254×9.5 12×10 305×254 0.375 9.53 0.349 8.86 14.6 9420 53 78.8
HSS 12×10×5/16 HSS 304.8×254×7.9 12×10 305×254 0.3125 7.94 0.291 7.39 12.2 7870 44.6 66.4
HSS 12×10×1/4 HSS 304.8×254×6.4 12×10 305×254 0.25 6.35 0.233 5.92 9.9 6390 36.03 53.6
HSS 12×8×5/8 HSS 304.8×203.2×15.9 12×8 305×203 0.625 15.9 0.581 14.8 21 13500 76.33 113
HSS 12×8×1/2 HSS 304.8×203.2×12.7 12×8 305×203 0.5 12.7 0.465 11.8 17.2 11100 62.46 92.7
HSS 12×8×3/8 HSS 304.8×203.2×9.5 12×8 305×203 0.375 9.53 0.349 8.86 13.2 8520 47.9 71.2
HSS 12×8×5/16 HSS 304.8×203.2×7.9 12×8 305×203 0.3125 7.94 0.291 7.39 11.1 7160 40.35 60.1
HSS 12×8×1/4 HSS 304.8×203.2×6.4 12×8 305×203 0.25 6.35 0.233 5.92 8.96 5780 32.63 48.5
HSS 12×8×3/16 HSS 304.8×203.2×4.8 12×8 305×203 0.1875 4.77 0.174 4.42 6.76 4360 24.73 36.9
HSS 12×6×5/8 HSS 304.8×152.4×15.9 12×6 305×152 0.625 15.9 0.581 14.8 18.7 12100 67.82 101
HSS 12×6×1/2 HSS 304.8×152.4×12.7 12×6 305×152 0.5 12.7 0.465 11.8 15.3 9870 55.66 82.6
HSS 12×6×3/8 HSS 304.8×152.4×9.5 12×6 305×152 0.375 9.53 0.349 8.86 11.8 7610 42.79 63.6
HSS 12×6×5/16 HSS 304.8×152.4×7.9 12×6 305×152 0.3125 7.94 0.291 7.39 9.92 6400 36.1 53.7
HSS 12×6×1/4 HSS 304.8×152.4×6.4 12×6 305×152 0.25 6.35 0.233 5.92 8.03 5180 29.23 43.4
HSS 12×6×3/16 HSS 304.8×152.4×4.8 12×6 305×152 0.1875 4.76 0.174 4.42 6.06 3910 22.18 33.1
HSS 12×4×5/8 HSS 304.8×101.6×15.9 12×4 305×102 0.625 15.9 0.581 14.8 16.4 10600 59.32 88
HSS 12×4×1/2 HSS 304.8×101.6×12.7 12×4 305×102 0.5 12.7 0.465 11.8 13.5 8710 48.85 72.5
HSS 12×4×3/8 HSS 304.8×101.6×9.5 12×4 305×102 0.375 9.53 0.349 8.86 10.4 6710 37.69 56
HSS 12×4×5/16 HSS 304.8×101.6×7.9 12×4 305×102 0.3125 7.94 0.291 7.39 8.76 5650 31.84 47.4
HSS 12×4×1/4 HSS 304.8×101.6×6.4 12×4 305×102 0.25 6.35 0.233 5.92 7.1 4580 25.82 38.4
HSS 12×4×3/16 HSS 304.8×101.6×4.8 12×4 305×102 0.1875 4.76 0.174 4.42 5.37 3460 19.63 29.3
HSS 12×3-1/2×3/8 HSS 304.8×88.9×9.5 12×3.5 305×88.9 0.375 9.53 0.349 8.86 10 6450 36.41 54.1
HSS 12×3-1/2×5/16 HSS 304.8×88.9×7.9 12×3.5 305×88.9 0.3125 7.94 0.291 7.39 8.46 5460 30.78 45.8
HSS 12×3×5/16 HSS 304.8×76.2×7.9 12×3 305×76.2 0.3125 7.94 0.291 7.39 8.17 5270 29.72 44.2
HSS 12×3×1/4 HSS 304.8×76.2×6.4 12×3 305×76.2 0.25 6.35 0.233 5.92 6.63 4280 24.12 35.8
HSS 12×3×3/16 HSS 304.8×76.2×4.8 12×3 305×76.2 0.1875 4.76 0.174 4.42 5.02 3240 18.35 27.4
HSS 12×2×5/16 HSS 304.8×50.8×7.9 12×2 305×50.8 0.3125 7.94 0.291 7.39 7.59 4900 27.59 41
HSS 12×2×1/4 HSS 304.8×50.8×6.4 12×2 305×50.8 0.25 6.35 0.233 5.92 6.17 3980 22.42 33.3
HSS 12×2×3/16 HSS 304.8×50.8×4.8 12×2 305×50.8 0.1875 4.76 0.174 4.42 4.67 3010 17.08 25.4
HSS 10×8×5/8 HSS 254×203.2×15.9 10×8 254×203 0.625 15.9 0.581 14.8 18.7 12100 67.82 101
HSS 10×8×1/2 HSS 254×203.2×12.7 10×8 254×203 0.5 12.7 0.465 11.8 15.3 9870 55.66 82.6
HSS 10×8×3/8 HSS 254×203.2×9.5 10×8 254×203 0.375 9.53 0.349 8.86 11.8 7610 42.79 63.6
HSS 10×8×5/16 HSS 254×203.2×7.9 10×8 254×203 0.3125 7.94 0.291 7.39 9.92 6400 36.1 53.7
HSS 10×8×1/4 HSS 254×203.2×6.4 10×8 254×203 0.25 6.35 0.233 5.92 8.03 5180 29.23 43.4
HSS 10×8×3/16 HSS 254×203.2×4.8 10×8 254×203 0.1875 4.76 0.174 4.42 6.06 3910 22.18 33.1
HSS 10×6×5/8 HSS 254×152.4×15.9 10×6 254×152 0.625 15.9 0.581 14.8 16.4 10600 59.32 88
HSS 10×6×1/2 HSS 254×152.4×12.7 10×6 254×152 0.5 12.7 0.465 11.8 13.5 8710 48.85 72.5
HSS 10×6×3/8 HSS 254×152.4×9.5 10×6 254×152 0.375 9.53 0.349 8.86 10.4 6710 37.69 56
HSS 10×6×5/16 HSS 254×152.4×7.9 10×6 254×152 0.3125 7.94 0.291 7.39 8.76 5650 31.84 47.4
HSS 10×6×1/4 HSS 254×152.4×6.4 10×6 254×152 0.25 6.35 0.233 5.92 7.1 4580 25.82 38.4
HSS 10×6×3/16 HSS 254×152.4×4.8 10×6 254×152 0.1875 4.76 0.174 4.42 5.37 3460 19.63 29.3
HSS 10×5×3/8 HSS 254×127×9.5 10×5 254×127 0.375 9.53 0.349 8.86 9.67 6240 35.13 52.2
HSS 10×5×5/16 HSS 254×127×7.9 10×5 254×127 0.3125 7.94 0.291 7.39 8.17 5270 29.72 44.2
HSS 10×5×1/4 HSS 254×127×6.4 10×5 254×127 0.25 6.35 0.233 5.92 6.63 4280 24.12 35.8
HSS 10×5×3/16 HSS 254×127×4.8 10×5 254×127 0.1875 4.76 0.174 4.42 5.02 3240 18.35 27.4
HSS 10×4×5/8 HSS 254×101.6×15.9 10×4 254×102 0.625 15.9 0.581 14.8 14 9030 50.81 75.3
HSS 10×4×1/2 HSS 254×101.6×12.7 10×4 254×102 0.5 12.7 0.465 11.8 11.6 7480 42.05 62.4
HSS 10×4×3/8 HSS 254×101.6×9.5 10×4 254×102 0.375 9.53 0.349 8.86 8.97 5790 32.58 48.4
HSS 10×4×5/16 HSS 254×101.6×7.9 10×4 254×102 0.3125 7.94 0.291 7.39 7.59 4900 27.59 41
HSS 10×4×1/4 HSS 254×101.6×6.4 10×4 254×102 0.25 6.35 0.233 5.92 6.17 3980 22.42 33.3
HSS 10×4×3/16 HSS 254×101.6×4.8 10×4 254×102 0.1875 4.76 0.174 4.42 4.67 3010 17.08 25.4
HSS 10×4×1/8 HSS 254×101.6×3.2 10×4 254×102 0.125 3.18 0.116 2.95 3.16 2040 11.56 17.2
HSS 10×3-1/2×1/2 HSS 254×88.9×12.7 10×3.5 254×88.9 0.5 12.7 0.465 11.8 11.1 7160 40.34 59.8
HSS 10×3-1/2×3/8 HSS 254×88.9×9.5 10×3.5 254×88.9 0.375 9.53 0.349 8.86 8.62 5560 31.31 46.5
HSS 10×3-1/2×5/16 HSS 254×88.9×7.9 10×3.5 254×88.9 0.3125 7.94 0.291 7.39 7.3 4710 26.53 39.5
HSS 10×3-1/2×1/4 HSS 254×88.9×6.4 10×3.5 254×88.9 0.25 6.35 0.233 5.92 5.93 3830 21.57 32
HSS 10×3-1/2×3/16 HSS 254×88.9×4.8 10×3.5 254×88.9 0.1875 4.76 0.174 4.42 4.5 2900 16.44 24.5
HSS 10×3-1/2×1/8 HSS 254×88.9×3.2 10×3.5 254×88.9 0.125 3.18 0.116 2.95 3.04 1960 11.13 16.6
HSS 10×3×3/8 HSS 254×76.2×9.5 10×3 254×76.2 0.375 9.53 0.349 8.86 8.27 5340 30.03 44.6
HSS 10×3×5/16 HSS 254×76.2×7.9 10×3 254×76.2 0.3125 7.94 0.291 7.39 7.01 4520 25.46 37.9
HSS 10×3×1/4 HSS 254×76.2×6.4 10×3 254×76.2 0.25 6.35 0.233 5.92 5.7 3680 20.72 30.8
HSS 10×3×3/16 HSS 254×76.2×4.8 10×3 254×76.2 0.1875 4.76 0.174 4.42 4.32 2790 15.8 23.5
HSS 10×3×1/8 HSS 254×76.2×3.2 10×3 254×76.2 0.125 3.18 0.116 2.95 2.93 1890 10.71 15.9
HSS 10×2×3/8 HSS 254×50.8×9.5 10×2 254×50.8 0.375 9.53 0.349 8.86 7.58 4890 27.48 40.8
HSS 10×2×5/16 HSS 254×50.8×7.9 10×2 254×50.8 0.3125 7.94 0.291 7.39 6.43 4150 23.34 34.7
HSS 10×2×1/4 HSS 254×50.8×6.4 10×2 254×50.8 0.25 6.35 0.233 5.92 5.24 3380 19.02 28.3
HSS 10×2×3/16 HSS 254×50.8×4.8 10×2 254×50.8 0.1875 4.76 0.174 4.42 3.98 2570 14.53 21.6
HSS 10×2×1/8 HSS 254×50.8×3.2 10×2 254×50.8 0.125 3.18 0.116 2.95 2.7 1740 9.86 14.7

HSS 9×… to HSS 7×…

62 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation H×B (in) H×B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 9×7×5/8 HSS 228.6×177.8×15.9 9×7 229×178 0.625 15.9 0.581 14.8 16.4 10600 59.32 88
HSS 9×7×1/2 HSS 228.6×177.8×12.7 9×7 229×178 0.5 12.7 0.465 11.8 13.5 8710 48.85 72.5
HSS 9×7×3/8 HSS 228.6×177.8×9.5 9×7 229×178 0.375 9.53 0.349 8.86 10.4 6710 37.69 56
HSS 9×7×5/16 HSS 228.6×177.8×7.9 9×7 229×178 0.3125 7.94 0.291 7.39 8.76 5650 31.84 47.4
HSS 9×7×1/4 HSS 228.6×177.8×6.4 9×7 229×178 0.25 6.35 0.233 5.92 7.1 4580 25.82 38.4
HSS 9×7×3/16 HSS 228.6×177.8×4.8 9×7 229×178 0.1875 4.76 0.174 4.42 5.37 3460 19.63 29.3
HSS 9×5×5/8 HSS 228.6×127×15.9 9×5 229×127 0.625 15.9 0.581 14.8 14 9030 50.81 75.3
HSS 9×5×1/2 HSS 228.6×127×12.7 9×5 229×127 0.5 12.7 0.465 11.8 11.6 7480 42.05 62.4
HSS 9×5×3/8 HSS 228.6×127×9.5 9×5 229×127 0.375 9.53 0.349 8.86 8.97 5790 32.58 48.4
HSS 9×5×5/16 HSS 228.6×127×7.9 9×5 229×127 0.3125 7.94 0.291 7.39 7.59 4900 27.59 41
HSS 9×5×1/4 HSS 228.6×127×6.4 9×5 229×127 0.25 6.35 0.233 5.92 6.17 3980 22.42 33.3
HSS 9×5×3/16 HSS 228.6×127×4.8 9×5 229×127 0.1875 4.76 0.174 4.42 4.67 3010 17.08 25.4
HSS 9×3×1/2 HSS 228.6×76.2×12.7 9×3 229×76.2 0.5 12.7 0.465 11.8 9.74 6280 35.24 52.2
HSS 9×3×3/8 HSS 228.6×76.2×9.5 9×3 229×76.2 0.375 9.53 0.349 8.86 7.58 4890 27.48 40.8
HSS 9×3×5/16 HSS 228.6×76.2×7.9 9×3 229×76.2 0.3125 7.94 0.291 7.39 6.43 4150 23.34 34.7
HSS 9×3×1/4 HSS 228.6×76.2×6.4 9×3 229×76.2 0.25 6.35 0.233 5.92 5.24 3380 19.02 28.3
HSS 9×3×3/16 HSS 228.6×76.2×4.8 9×3 229×76.2 0.1875 4.76 0.174 4.42 3.98 2570 14.53 21.6
HSS 8×6×5/8 HSS 203.2×152.4×15.9 8×6 203×152 0.625 15.9 0.581 14.8 14 9030 50.81 75.3
HSS 8×6×1/2 HSS 203.2×152.4×12.7 8×6 203×152 0.5 12.7 0.465 11.8 11.6 7480 42.05 62.4
HSS 8×6×3/8 HSS 203.2×152.4×9.5 8×6 203×152 0.375 9.53 0.349 8.86 8.97 5790 32.58 48.4
HSS 8×6×5/16 HSS 203.2×152.4×7.9 8×6 203×152 0.3125 7.94 0.291 7.39 7.59 4900 27.59 41
HSS 8×6×1/4 HSS 203.2×152.4×6.4 8×6 203×152 0.25 6.35 0.233 5.92 6.17 3980 22.42 33.3
HSS 8×6×3/16 HSS 203.2×152.4×4.8 8×6 203×152 0.1875 4.76 0.174 4.42 4.67 3010 17.08 25.4
HSS 8×4×5/8 HSS 203.2×101.6×15.9 8×4 203×102 0.625 15.9 0.581 14.8 11.7 7550 42.3 62.6
HSS 8×4×1/2 HSS 203.2×101.6×12.7 8×4 203×102 0.5 12.7 0.465 11.8 9.74 6280 35.24 52.2
HSS 8×4×3/8 HSS 203.2×101.6×9.5 8×4 203×102 0.375 9.53 0.349 8.86 7.58 4890 27.48 40.8
HSS 8×4×5/16 HSS 203.2×101.6×7.9 8×4 203×102 0.3125 7.94 0.291 7.39 6.43 4150 23.34 34.7
HSS 8×4×1/4 HSS 203.2×101.6×6.4 8×4 203×102 0.25 6.35 0.233 5.92 5.24 3380 19.02 28.3
HSS 8×4×3/16 HSS 203.2×101.6×4.8 8×4 203×102 0.1875 4.76 0.174 4.42 3.98 2570 14.53 21.6
HSS 8×4×1/8 HSS 203.2×101.6×3.2 8×4 203×102 0.125 3.18 0.116 2.95 2.7 1740 9.86 14.7
HSS 8×3×1/2 HSS 203.2×76.2×12.7 8×3 203×76.2 0.5 12.7 0.465 11.8 8.81 5680 31.84 47.2
HSS 8×3×3/8 HSS 203.2×76.2×9.5 8×3 203×76.2 0.375 9.53 0.349 8.86 6.88 4440 24.93 37
HSS 8×3×5/16 HSS 203.2×76.2×7.9 8×3 203×76.2 0.3125 7.94 0.291 7.39 5.85 3770 21.21 31.5
HSS 8×3×1/4 HSS 203.2×76.2×6.4 8×3 203×76.2 0.25 6.35 0.233 5.92 4.77 3080 17.32 25.7
HSS 8×3×3/16 HSS 203.2×76.2×4.8 8×3 203×76.2 0.1875 4.76 0.174 4.42 3.63 2340 13.25 19.7
HSS 8×3×1/8 HSS 203.2×76.2×3.2 8×3 203×76.2 0.125 3.18 0.116 2.95 2.46 1590 9.01 13.4
HSS 8×2×3/8 HSS 203.2×50.8×9.5 8×2 203×50.8 0.375 9.53 0.349 8.86 6.18 3990 22.37 33.2
HSS 8×2×5/16 HSS 203.2×50.8×7.9 8×2 203×50.8 0.3125 7.94 0.291 7.39 5.26 3390 19.08 28.4
HSS 8×2×1/4 HSS 203.2×50.8×6.4 8×2 203×50.8 0.25 6.35 0.233 5.92 4.3 2770 15.62 23.2
HSS 8×2×3/16 HSS 203.2×50.8×4.8 8×2 203×50.8 0.1875 4.76 0.174 4.42 3.28 2120 11.97 17.8
HSS 8×2×1/8 HSS 203.2×50.8×3.2 8×2 203×50.8 0.125 3.18 0.116 2.95 2.23 1440 8.16 12.1
HSS 7×5×1/2 HSS 177.8×127×12.7 7×5 178×127 0.5 12.7 0.465 11.8 9.74 6280 35.24 52.2
HSS 7×5×3/8 HSS 177.8×127×9.5 7×5 178×127 0.375 9.53 0.349 8.86 7.58 4890 27.48 40.8
HSS 7×5×5/16 HSS 177.8×127×7.9 7×5 178×127 0.3125 7.94 0.291 7.39 6.43 4150 23.34 34.7
HSS 7×5×1/4 HSS 177.8×127×6.4 7×5 178×127 0.25 6.35 0.233 5.92 5.24 3380 19.02 28.3
HSS 7×5×3/16 HSS 177.8×127×4.8 7×5 178×127 0.1875 4.76 0.174 4.42 3.98 2570 14.53 21.6
HSS 7×5×1/8 HSS 177.8×127×3.2 7×5 178×127 0.125 3.18 0.116 2.95 2.7 1740 9.86 14.7
HSS 7×4×1/2 HSS 177.8×101.6×12.7 7×4 178×102 0.5 12.7 0.465 11.8 8.81 5680 31.84 47.2
HSS 7×4×3/8 HSS 177.8×101.6×9.5 7×4 178×102 0.375 9.53 0.349 8.86 6.88 4440 24.93 37
HSS 7×4×5/16 HSS 177.8×101.6×7.9 7×4 178×102 0.3125 7.94 0.291 7.39 5.85 3770 21.21 31.5
HSS 7×4×1/4 HSS 177.8×101.6×6.4 7×4 178×102 0.25 6.35 0.233 5.92 4.77 3080 17.32 25.7
HSS 7×4×3/16 HSS 177.8×101.6×4.8 7×4 178×102 0.1875 4.76 0.174 4.42 3.63 2340 13.25 19.7
HSS 7×4×1/8 HSS 177.8×101.6×3.2 7×4 178×102 0.125 3.18 0.116 2.95 2.46 1590 9.01 13.4
HSS 7×3×1/2 HSS 177.8×76.2×12.7 7×3 178×76.2 0.5 12.7 0.465 11.8 7.88 5080 28.43 42.1
HSS 7×3×3/8 HSS 177.8×76.2×9.5 7×3 178×76.2 0.375 9.53 0.349 8.86 6.18 3990 22.37 33.2
HSS 7×3×5/16 HSS 177.8×76.2×7.9 7×3 178×76.2 0.3125 7.94 0.291 7.39 5.26 3390 19.08 28.4
HSS 7×3×1/4 HSS 177.8×76.2×6.4 7×3 178×76.2 0.25 6.35 0.233 5.92 4.3 2770 15.62 23.2
HSS 7×3×3/16 HSS 177.8×76.2×4.8 7×3 178×76.2 0.1875 4.76 0.174 4.42 3.28 2120 11.97 17.8
HSS 7×3×1/8 HSS 177.8×76.2×3.2 7×3 178×76.2 0.125 3.18 0.116 2.95 2.23 1440 8.16 12.1
HSS 7×2×1/4 HSS 177.8×50.8×6.4 7×2 178×50.8 0.25 6.35 0.233 5.92 3.84 2480 13.91 20.7
HSS 7×2×3/16 HSS 177.8×50.8×4.8 7×2 178×50.8 0.1875 4.76 0.174 4.42 2.93 1890 10.7 15.9
HSS 7×2×1/8 HSS 177.8×50.8×3.2 7×2 178×50.8 0.125 3.18 0.116 2.95 2 1290 7.31 10.9

HSS 6×… to HSS 5×…

43 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation H×B (in) H×B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 6×5×1/2 HSS 152.4×127×12.7 6×5 152×127 0.5 12.7 0.465 11.8 8.81 5680 31.84 47.2
HSS 6×5×3/8 HSS 152.4×127×9.5 6×5 152×127 0.375 9.53 0.349 8.86 6.88 4440 24.93 37
HSS 6×5×5/16 HSS 152.4×127×7.9 6×5 152×127 0.3125 7.94 0.291 7.39 5.85 3770 21.21 31.5
HSS 6×5×1/4 HSS 152.4×127×6.4 6×5 152×127 0.25 6.35 0.233 5.92 4.77 3080 17.32 25.7
HSS 6×5×3/16 HSS 152.4×127×4.8 6×5 152×127 0.1875 4.76 0.174 4.42 3.63 2340 13.25 19.7
HSS 6×5×1/8 HSS 152.4×127×3.2 6×5 152×127 0.125 3.18 0.116 2.95 2.46 1590 9.01 13.4
HSS 6×4×1/2 HSS 152.4×101.6×12.7 6×4 152×102 0.5 12.7 0.465 11.8 7.88 5080 28.43 42.1
HSS 6×4×3/8 HSS 152.4×101.6×9.5 6×4 152×102 0.375 9.53 0.349 8.86 6.18 3990 22.37 33.2
HSS 6×4×5/16 HSS 152.4×101.6×7.9 6×4 152×102 0.3125 7.94 0.291 7.39 5.26 3390 19.08 28.4
HSS 6×4×1/4 HSS 152.4×101.6×6.4 6×4 152×102 0.25 6.35 0.233 5.92 4.3 2770 15.62 23.2
HSS 6×4×3/16 HSS 152.4×101.6×4.8 6×4 152×102 0.1875 4.76 0.174 4.42 3.28 2120 11.97 17.8
HSS 6×4×1/8 HSS 152.4×101.6×3.2 6×4 152×102 0.125 3.18 0.116 2.95 2.23 1440 8.16 12.1
HSS 6×3×1/2 HSS 152.4×76.2×12.7 6×3 152×76.2 0.5 12.7 0.465 11.8 6.95 4480 25.03 37.1
HSS 6×3×3/8 HSS 152.4×76.2×9.5 6×3 152×76.2 0.375 9.53 0.349 8.86 5.48 3540 19.82 29.4
HSS 6×3×5/16 HSS 152.4×76.2×7.9 6×3 152×76.2 0.3125 7.94 0.291 7.39 4.68 3020 16.96 25.2
HSS 6×3×1/4 HSS 152.4×76.2×6.4 6×3 152×76.2 0.25 6.35 0.233 5.92 3.84 2480 13.91 20.7
HSS 6×3×3/16 HSS 152.4×76.2×4.8 6×3 152×76.2 0.1875 4.76 0.174 4.42 2.93 1890 10.7 15.9
HSS 6×3×1/8 HSS 152.4×76.2×3.2 6×3 152×76.2 0.125 3.18 0.116 2.95 2 1290 7.31 10.9
HSS 6×2×3/8 HSS 152.4×50.8×9.5 6×2 152×50.8 0.375 9.53 0.349 8.86 4.78 3080 17.27 25.6
HSS 6×2×5/16 HSS 152.4×50.8×7.9 6×2 152×50.8 0.3125 7.94 0.291 7.39 4.1 2650 14.83 22
HSS 6×2×1/4 HSS 152.4×50.8×6.4 6×2 152×50.8 0.25 6.35 0.233 5.92 3.37 2170 12.21 18.1
HSS 6×2×3/16 HSS 152.4×50.8×4.8 6×2 152×50.8 0.1875 4.76 0.174 4.42 2.58 1660 9.42 14
HSS 6×2×1/8 HSS 152.4×50.8×3.2 6×2 152×50.8 0.125 3.18 0.116 2.95 1.77 1140 6.46 9.59
HSS 5×4×1/2 HSS 127×101.6×12.7 5×4 127×102 0.5 12.7 0.465 11.8 6.95 4480 25.03 37.1
HSS 5×4×3/8 HSS 127×101.6×9.5 5×4 127×102 0.375 9.53 0.349 8.86 5.48 3540 19.82 29.4
HSS 5×4×5/16 HSS 127×101.6×7.9 5×4 127×102 0.3125 7.94 0.291 7.39 4.68 3020 16.96 25.2
HSS 5×4×1/4 HSS 127×101.6×6.4 5×4 127×102 0.25 6.35 0.233 5.92 3.84 2480 13.91 20.7
HSS 5×4×3/16 HSS 127×101.6×4.8 5×4 127×102 0.1875 4.76 0.174 4.42 2.93 1890 10.7 15.9
HSS 5×4×1/8 HSS 127×101.6×3.2 5×4 127×102 0.125 3.18 0.116 2.95 2 1290 7.31 10.9
HSS 5×3×1/2 HSS 127×76.2×12.7 5×3 127×76.2 0.5 12.7 0.465 11.8 6.02 3880 21.63 32
HSS 5×3×3/8 HSS 127×76.2×9.5 5×3 127×76.2 0.375 9.53 0.349 8.86 4.78 3080 17.27 25.6
HSS 5×3×5/16 HSS 127×76.2×7.9 5×3 127×76.2 0.3125 7.94 0.291 7.39 4.1 2650 14.83 22
HSS 5×3×1/4 HSS 127×76.2×6.4 5×3 127×76.2 0.25 6.35 0.233 5.92 3.37 2170 12.21 18.1
HSS 5×3×3/16 HSS 127×76.2×4.8 5×3 127×76.2 0.1875 4.76 0.174 4.42 2.58 1660 9.42 14
HSS 5×3×1/8 HSS 127×76.2×3.2 5×3 127×76.2 0.125 3.18 0.116 2.95 1.77 1140 6.46 9.59
HSS 5×2-1/2×1/4 HSS 127×63.5×6.4 5×2.5 127×63.5 0.25 6.35 0.233 5.92 3.14 2030 11.36 16.9
HSS 5×2-1/2×3/16 HSS 127×63.5×4.8 5×2.5 127×63.5 0.1875 4.76 0.174 4.42 2.41 1550 8.78 13.1
HSS 5×2-1/2×1/8 HSS 127×63.5×3.2 5×2.5 127×63.5 0.125 3.18 0.116 2.95 1.65 1060 6.03 8.96
HSS 5×2×3/8 HSS 127×50.8×9.5 5×2 127×50.8 0.375 9.53 0.349 8.86 4.09 2640 14.72 21.8
HSS 5×2×5/16 HSS 127×50.8×7.9 5×2 127×50.8 0.3125 7.94 0.291 7.39 3.52 2270 12.7 18.8
HSS 5×2×1/4 HSS 127×50.8×6.4 5×2 127×50.8 0.25 6.35 0.233 5.92 2.91 1880 10.51 15.6
HSS 5×2×3/16 HSS 127×50.8×4.8 5×2 127×50.8 0.1875 4.76 0.174 4.42 2.24 1450 8.15 12.1
HSS 5×2×1/8 HSS 127×50.8×3.2 5×2 127×50.8 0.125 3.18 0.116 2.95 1.54 994 5.61 8.33

HSS 4.5×… to HSS 2×…

53 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation H×B (in) H×B (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 4×3×3/8 HSS 101.6×76.2×9.5 4×3 102×76.2 0.375 9.53 0.349 8.86 4.09 2640 14.72 21.8
HSS 4×3×5/16 HSS 101.6×76.2×7.9 4×3 102×76.2 0.3125 7.94 0.291 7.39 3.52 2270 12.7 18.8
HSS 4×3×1/4 HSS 101.6×76.2×6.4 4×3 102×76.2 0.25 6.35 0.233 5.92 2.91 1880 10.51 15.6
HSS 4×3×3/16 HSS 101.6×76.2×4.8 4×3 102×76.2 0.1875 4.76 0.174 4.42 2.24 1450 8.15 12.1
HSS 4×3×1/8 HSS 101.6×76.2×3.2 4×3 102×76.2 0.125 3.18 0.116 2.95 1.54 994 5.61 8.33
HSS 4×2-1/2×3/8 HSS 101.6×63.5×9.5 4×2.5 102×63.5 0.375 9.53 0.349 8.86 3.74 2410 13.44 19.9
HSS 4×2-1/2×5/16 HSS 101.6×63.5×7.9 4×2.5 102×63.5 0.3125 7.94 0.291 7.39 3.23 2080 11.64 17.3
HSS 4×2-1/2×1/4 HSS 101.6×63.5×6.4 4×2.5 102×63.5 0.25 6.35 0.233 5.92 2.67 1720 9.66 14.3
HSS 4×2-1/2×3/16 HSS 101.6×63.5×4.8 4×2.5 102×63.5 0.1875 4.76 0.174 4.42 2.06 1330 7.51 11.2
HSS 4×2-1/2×1/8 HSS 101.6×63.5×3.2 4×2.5 102×63.5 0.125 3.18 0.116 2.95 1.42 916 5.18 7.7
HSS 4×2×3/8 HSS 101.6×50.8×9.5 4×2 102×50.8 0.375 9.53 0.349 8.86 3.39 2190 12.17 18
HSS 4×2×5/16 HSS 101.6×50.8×7.9 4×2 102×50.8 0.3125 7.94 0.291 7.39 2.94 1900 10.58 15.7
HSS 4×2×1/4 HSS 101.6×50.8×6.4 4×2 102×50.8 0.25 6.35 0.233 5.92 2.44 1570 8.81 13.1
HSS 4×2×3/16 HSS 101.6×50.8×4.8 4×2 102×50.8 0.1875 4.76 0.174 4.42 1.89 1220 6.87 10.2
HSS 4×2×1/8 HSS 101.6×50.8×3.2 4×2 102×50.8 0.125 3.18 0.116 2.95 1.3 839 4.75 7.06
HSS 3-1/2×2-1/2×3/8 HSS 88.9×63.5×9.5 3.5×2.5 88.9×63.5 0.375 9.53 0.349 8.86 3.39 2190 12.17 18
HSS 3-1/2×2-1/2×5/16 HSS 88.9×63.5×7.9 3.5×2.5 88.9×63.5 0.3125 7.94 0.291 7.39 2.94 1900 10.58 15.6
HSS 3-1/2×2-1/2×1/4 HSS 88.9×63.5×6.4 3.5×2.5 88.9×63.5 0.25 6.35 0.233 5.92 2.44 1570 8.81 13.1
HSS 3-1/2×2-1/2×3/16 HSS 88.9×63.5×4.8 3.5×2.5 88.9×63.5 0.1875 4.76 0.174 4.42 1.89 1220 6.87 10.2
HSS 3-1/2×2-1/2×1/8 HSS 88.9×63.5×3.2 3.5×2.5 88.9×63.5 0.125 3.18 0.116 2.95 1.3 839 4.75 7.07
HSS 3-1/2×2×1/4 HSS 88.9×50.8×6.4 3.5×2 88.9×50.8 0.25 6.35 0.233 5.92 2.21 1430 7.96 11.8
HSS 3-1/2×2×3/16 HSS 88.9×50.8×4.8 3.5×2 88.9×50.8 0.1875 4.76 0.174 4.42 1.71 1100 6.23 9.27
HSS 3-1/2×2×1/8 HSS 88.9×50.8×3.2 3.5×2 88.9×50.8 0.125 3.18 0.116 2.95 1.19 768 4.33 6.43
HSS 3-1/2×1-1/2×1/4 HSS 88.9×38.1×6.4 3.5×1.5 88.9×38.1 0.25 6.35 0.233 5.92 1.97 1270 7.11 10.5
HSS 3-1/2×1-1/2×3/16 HSS 88.9×38.1×4.8 3.5×1.5 88.9×38.1 0.1875 4.76 0.174 4.42 1.54 994 5.59 8.31
HSS 3-1/2×1-1/2×1/8 HSS 88.9×38.1×3.2 3.5×1.5 88.9×38.1 0.125 3.18 0.116 2.95 1.07 690 3.9 5.8
HSS 3×2-1/2×5/16 HSS 76.2×63.5×7.9 3×2.5 76.2×63.5 0.3125 7.94 0.291 7.39 2.64 1700 9.51 14.1
HSS 3×2-1/2×1/4 HSS 76.2×63.5×6.4 3×2.5 76.2×63.5 0.25 6.35 0.233 5.92 2.21 1430 7.96 11.8
HSS 3×2-1/2×3/16 HSS 76.2×63.5×4.8 3×2.5 76.2×63.5 0.1875 4.76 0.174 4.42 1.71 1100 6.23 9.27
HSS 3×2-1/2×1/8 HSS 76.2×63.5×3.2 3×2.5 76.2×63.5 0.125 3.18 0.116 2.95 1.19 768 4.33 6.43
HSS 3×2×5/16 HSS 76.2×50.8×7.9 3×2 76.2×50.8 0.3125 7.94 0.291 7.39 2.35 1520 8.45 12.5
HSS 3×2×1/4 HSS 76.2×50.8×6.4 3×2 76.2×50.8 0.25 6.35 0.233 5.92 1.97 1270 7.11 10.5
HSS 3×2×3/16 HSS 76.2×50.8×4.8 3×2 76.2×50.8 0.1875 4.76 0.174 4.42 1.54 994 5.59 8.31
HSS 3×2×1/8 HSS 76.2×50.8×3.2 3×2 76.2×50.8 0.125 3.18 0.116 2.95 1.07 690 3.9 5.8
HSS 3×1-1/2×1/4 HSS 76.2×38.1×6.4 3×1.5 76.2×38.1 0.25 6.35 0.233 5.92 1.74 1120 6.26 9.26
HSS 3×1-1/2×3/16 HSS 76.2×38.1×4.8 3×1.5 76.2×38.1 0.1875 4.76 0.174 4.42 1.37 884 4.96 7.36
HSS 3×1-1/2×1/8 HSS 76.2×38.1×3.2 3×1.5 76.2×38.1 0.125 3.18 0.116 2.95 0.956 617 3.48 5.16
HSS 3×1×3/16 HSS 76.2×25.4×4.8 3×1 76.2×25.4 0.1875 4.76 0.174 4.42 1.19 768 4.32 6.41
HSS 3×1×1/8 HSS 76.2×25.4×3.2 3×1 76.2×25.4 0.125 3.18 0.116 2.95 0.84 542 3.05 4.53
HSS 2-1/2×2×1/4 HSS 63.5×50.8×6.4 2.5×2 63.5×50.8 0.25 6.35 0.233 5.92 1.74 1120 6.26 9.26
HSS 2-1/2×2×3/16 HSS 63.5×50.8×4.8 2.5×2 63.5×50.8 0.1875 4.76 0.174 4.42 1.37 884 4.96 7.36
HSS 2-1/2×2×1/8 HSS 63.5×50.8×3.2 2.5×2 63.5×50.8 0.125 3.18 0.116 2.95 0.956 617 3.48 5.16
HSS 2-1/2×1-1/2×1/4 HSS 63.5×38.1×6.4 2.5×1.5 63.5×38.1 0.25 6.35 0.233 5.92 1.51 974 5.41 8
HSS 2-1/2×1-1/2×3/16 HSS 63.5×38.1×4.8 2.5×1.5 63.5×38.1 0.1875 4.76 0.174 4.42 1.19 768 4.32 6.41
HSS 2-1/2×1-1/2×1/8 HSS 63.5×38.1×3.2 2.5×1.5 63.5×38.1 0.125 3.18 0.116 2.95 0.84 542 3.05 4.53
HSS 2-1/2×1×3/16 HSS 63.5×25.4×4.8 2.5×1 63.5×25.4 0.1875 4.76 0.174 4.42 1.02 658 3.68 5.46
HSS 2-1/2×1×1/8 HSS 63.5×25.4×3.2 2.5×1 63.5×25.4 0.125 3.18 0.116 2.95 0.724 467 2.63 3.9
HSS 2-1/4×2×3/16 HSS 57.2×50.8×4.8 2.25×2 57.2×50.8 0.1875 4.76 0.174 4.42 1.28 826 4.64 6.89
HSS 2-1/4×2×1/8 HSS 57.2×50.8×3.2 2.25×2 57.2×50.8 0.125 3.18 0.116 2.95 0.898 579 3.27 4.85
HSS 2×1-1/2×3/16 HSS 50.8×38.1×4.8 2×1.5 50.8×38.1 0.1875 4.76 0.174 4.42 1.02 658 3.68 5.46
HSS 2×1-1/2×1/8 HSS 50.8×38.1×3.2 2×1.5 50.8×38.1 0.125 3.18 0.116 2.95 0.724 467 2.63 3.9
HSS 2×1×3/16 HSS 50.8×25.4×4.8 2×1 50.8×25.4 0.1875 4.76 0.174 4.42 0.845 545 3.04 4.51
HSS 2×1×1/8 HSS 50.8×25.4×3.2 2×1 50.8×25.4 0.125 3.18 0.116 2.95 0.608 392 2.2 3.26

Round HSS (CHS)

128 round designations, grouped by outside diameter. These are HSS, not AISC Pipe and not ASTM A53 pipe, even when the outside diameter looks familiar.

HSS 20.000 to HSS 10.000

27 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation OD (in) OD (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 20.000×0.500 HSS 508×12.7 20 508 0.5 12.7 0.465 11.8 28.5 18400 104 155
HSS 20.000×0.375 HSS 508×9.5 20 508 0.375 9.53 0.349 8.86 21.5 13900 78.67 117
HSS 18.000×0.500 HSS 457.2×12.7 18 457 0.5 12.7 0.465 11.8 25.6 16500 93.54 139
HSS 18.000×0.375 HSS 457.2×9.5 18 457 0.375 9.53 0.349 8.86 19.4 12500 70.66 105
HSS 16.000×0.625 HSS 406.4×15.9 16 406 0.625 15.9 0.581 14.8 28.1 18100 103 153
HSS 16.000×0.500 HSS 406.4×12.7 16 406 0.5 12.7 0.465 11.8 22.7 14600 82.85 123
HSS 16.000×0.438 HSS 406.4×11.1 16 406 0.438 11.1 0.407 10.3 19.9 12800 72.87 108
HSS 16.000×0.375 HSS 406.4×9.5 16 406 0.375 9.53 0.349 8.86 17.2 11100 62.64 93.2
HSS 16.000×0.312 HSS 406.4×7.9 16 406 0.312 7.94 0.291 7.39 14.4 9290 52.32 77.9
HSS 16.000×0.250 HSS 406.4×6.4 16 406 0.25 6.35 0.233 5.92 11.5 7420 42.09 62.6
HSS 14.000×0.625 HSS 355.6×15.9 14 356 0.625 15.9 0.581 14.8 24.5 15800 89.36 133
HSS 14.000×0.500 HSS 355.6×12.7 14 356 0.5 12.7 0.465 11.8 19.8 12800 72.16 107
HSS 14.000×0.375 HSS 355.6×9.5 14 356 0.375 9.53 0.349 8.86 15 9680 54.62 81.3
HSS 14.000×0.312 HSS 355.6×7.9 14 356 0.312 7.94 0.291 7.39 12.5 8060 45.65 67.9
HSS 14.000×0.250 HSS 355.6×6.4 14 356 0.25 6.35 0.233 5.92 10.1 6520 36.75 54.7
HSS 12.750×0.500 HSS 323.9×12.7 12.8 324 0.5 12.7 0.465 11.8 17.9 11500 65.48 97.4
HSS 12.750×0.375 HSS 323.9×9.5 12.8 324 0.375 9.53 0.349 8.86 13.6 8770 49.61 73.8
HSS 12.750×0.250 HSS 323.9×6.4 12.8 324 0.25 6.35 0.233 5.92 9.16 5910 33.41 49.7
HSS 10.750×0.500 HSS 273.1×12.7 10.8 273 0.5 12.7 0.465 11.8 15 9680 54.79 81.5
HSS 10.750×0.375 HSS 273.1×9.5 10.8 273 0.375 9.53 0.349 8.86 11.4 7350 41.59 61.9
HSS 10.750×0.250 HSS 273.1×6.4 10.8 273 0.25 6.35 0.233 5.92 7.7 4970 28.06 41.8
HSS 10.000×0.625 HSS 254×15.9 10 254 0.625 15.9 0.581 14.8 17.2 11100 62.64 93.2
HSS 10.000×0.500 HSS 254×12.7 10 254 0.5 12.7 0.465 11.8 13.9 8970 50.78 75.6
HSS 10.000×0.375 HSS 254×9.5 10 254 0.375 9.53 0.349 8.86 10.6 6840 38.58 57.4
HSS 10.000×0.312 HSS 254×7.9 10 254 0.312 7.94 0.291 7.39 8.88 5730 32.31 48.1
HSS 10.000×0.250 HSS 254×6.4 10 254 0.25 6.35 0.233 5.92 7.15 4610 26.06 38.8
HSS 10.000×0.188 HSS 254×4.8 10 254 0.188 4.78 0.174 4.42 5.37 3460 19.72 29.3

HSS 9.625 to HSS 5.563

49 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation OD (in) OD (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 9.625×0.500 HSS 244.5×12.7 9.63 244 0.5 12.7 0.465 11.8 13.4 8650 48.77 72.6
HSS 9.625×0.375 HSS 244.5×9.5 9.63 244 0.375 9.53 0.349 8.86 10.2 6580 37.08 55.2
HSS 9.625×0.312 HSS 244.5×7.9 9.63 244 0.312 7.94 0.291 7.39 8.53 5500 31.06 46.2
HSS 9.625×0.250 HSS 244.5×6.4 9.63 244 0.25 6.35 0.233 5.92 6.87 4430 25.06 37.3
HSS 9.625×0.188 HSS 244.5×4.8 9.63 244 0.188 4.78 0.174 4.42 5.17 3340 18.97 28.2
HSS 8.625×0.625 HSS 219.1×15.9 8.63 219 0.625 15.9 0.581 14.8 14.7 9480 53.45 79.5
HSS 8.625×0.500 HSS 219.1×12.7 8.63 219 0.5 12.7 0.465 11.8 11.9 7680 43.43 64.6
HSS 8.625×0.375 HSS 219.1×9.5 8.63 219 0.375 9.53 0.349 8.86 9.07 5850 33.07 49.2
HSS 8.625×0.322 HSS 219.1×8.2 8.63 219 0.322 8.18 0.3 7.62 7.85 5060 28.58 42.5
HSS 8.625×0.250 HSS 219.1×6.4 8.63 219 0.25 6.35 0.233 5.92 6.14 3960 22.38 33.3
HSS 8.625×0.188 HSS 219.1×4.8 8.63 219 0.188 4.78 0.174 4.42 4.62 2980 16.96 25.2
HSS 7.625×0.375 HSS 193.7×9.5 7.63 194 0.375 9.53 0.349 8.86 7.98 5150 29.06 43.2
HSS 7.625×0.328 HSS 193.7×8.3 7.63 194 0.328 8.33 0.305 7.75 7.01 4520 25.59 38.1
HSS 7.500×0.500 HSS 190.5×12.7 7.5 191 0.5 12.7 0.465 11.8 10.3 6650 37.42 55.7
HSS 7.500×0.375 HSS 190.5×9.5 7.5 191 0.375 9.53 0.349 8.86 7.84 5060 28.56 42.5
HSS 7.500×0.312 HSS 190.5×7.9 7.5 191 0.312 7.94 0.291 7.39 6.59 4250 23.97 35.7
HSS 7.500×0.250 HSS 190.5×6.4 7.5 191 0.25 6.35 0.233 5.92 5.32 3430 19.38 28.8
HSS 7.500×0.188 HSS 190.5×4.8 7.5 191 0.188 4.78 0.174 4.42 4 2580 14.7 21.9
HSS 7.000×0.500 HSS 177.8×12.7 7 178 0.5 12.7 0.465 11.8 9.55 6160 34.74 51.7
HSS 7.000×0.375 HSS 177.8×9.5 7 178 0.375 9.53 0.349 8.86 7.29 4700 26.56 39.5
HSS 7.000×0.312 HSS 177.8×7.9 7 178 0.312 7.94 0.291 7.39 6.13 3950 22.31 33.2
HSS 7.000×0.250 HSS 177.8×6.4 7 178 0.25 6.35 0.233 5.92 4.95 3190 18.04 26.8
HSS 7.000×0.188 HSS 177.8×4.8 7 178 0.188 4.78 0.174 4.42 3.73 2410 13.69 20.4
HSS 7.000×0.125 HSS 177.8×3.2 7 178 0.125 3.18 0.116 2.95 2.51 1620 9.19 13.7
HSS 6.875×0.500 HSS 174.6×12.7 6.88 175 0.5 12.7 0.465 11.8 9.36 6040 34.07 50.7
HSS 6.875×0.375 HSS 174.6×9.5 6.88 175 0.375 9.53 0.349 8.86 7.16 4620 26.06 38.8
HSS 6.875×0.312 HSS 174.6×7.9 6.88 175 0.312 7.94 0.291 7.39 6.02 3880 21.89 32.6
HSS 6.875×0.250 HSS 174.6×6.4 6.88 175 0.25 6.35 0.233 5.92 4.86 3140 17.71 26.3
HSS 6.875×0.188 HSS 174.6×4.8 6.88 175 0.188 4.78 0.174 4.42 3.66 2360 13.44 20
HSS 6.625×0.500 HSS 168.3×12.7 6.63 168 0.5 12.7 0.465 11.8 9 5810 32.74 48.7
HSS 6.625×0.432 HSS 168.3×11 6.63 168 0.432 11.1 0.402 10.2 7.86 5070 28.6 42.6
HSS 6.625×0.375 HSS 168.3×9.5 6.63 168 0.375 9.53 0.349 8.86 6.88 4440 25.06 37.3
HSS 6.625×0.312 HSS 168.3×7.9 6.63 168 0.312 7.94 0.291 7.39 5.79 3740 21.06 31.3
HSS 6.625×0.280 HSS 168.3×7.1 6.63 168 0.28 7.11 0.26 6.6 5.2 3350 18.99 28.3
HSS 6.625×0.250 HSS 168.3×6.4 6.63 168 0.25 6.35 0.233 5.92 4.68 3020 17.04 25.4
HSS 6.625×0.188 HSS 168.3×4.8 6.63 168 0.188 4.78 0.174 4.42 3.53 2280 12.94 19.2
HSS 6.625×0.125 HSS 168.3×3.2 6.63 168 0.125 3.18 0.116 2.95 2.37 1530 8.69 12.9
HSS 6.000×0.500 HSS 152.4×12.7 6 152 0.5 12.7 0.465 11.8 8.09 5220 29.4 43.7
HSS 6.000×0.375 HSS 152.4×9.5 6 152 0.375 9.53 0.349 8.86 6.2 4000 22.55 33.6
HSS 6.000×0.312 HSS 152.4×7.9 6 152 0.312 7.94 0.291 7.39 5.22 3370 18.97 28.2
HSS 6.000×0.280 HSS 152.4×7.1 6 152 0.28 7.11 0.26 6.6 4.69 3030 17.12 25.5
HSS 6.000×0.250 HSS 152.4×6.4 6 152 0.25 6.35 0.233 5.92 4.22 2720 15.37 22.9
HSS 6.000×0.188 HSS 152.4×4.8 6 152 0.188 4.78 0.174 4.42 3.18 2050 11.68 17.4
HSS 6.000×0.125 HSS 152.4×3.2 6 152 0.125 3.18 0.116 2.95 2.14 1380 7.85 11.7
HSS 5.563×0.500 HSS 141.3×12.7 5.56 141 0.5 12.7 0.465 11.8 7.45 4810 27.06 40.3
HSS 5.563×0.375 HSS 141.3×9.5 5.56 141 0.375 9.53 0.349 8.86 5.72 3690 20.8 30.9
HSS 5.563×0.258 HSS 141.3×6.6 5.56 141 0.258 6.55 0.24 6.1 4.01 2590 14.63 21.8
HSS 5.563×0.188 HSS 141.3×4.8 5.56 141 0.188 4.78 0.174 4.42 2.95 1900 10.8 16.1
HSS 5.563×0.134 HSS 141.3×3.4 5.56 141 0.134 3.4 0.124 3.15 2.12 1370 7.78 11.6

HSS 5.000 to HSS 1.660

52 designations in this group.

Swipe horizontally to view all dimensions.

Designation SI designation OD (in) OD (mm) tnom (in) tnom (mm) tdes (in) tdes (mm) A (in²) A (mm²) Mass (lb/ft) Mass (kg/m)
HSS 5.500×0.500 HSS 139.7×12.7 5.5 140 0.5 12.7 0.465 11.8 7.36 4750 26.73 39.8
HSS 5.500×0.375 HSS 139.7×9.5 5.5 140 0.375 9.53 0.349 8.86 5.65 3650 20.55 30.6
HSS 5.500×0.258 HSS 139.7×6.6 5.5 140 0.258 6.55 0.24 6.1 3.97 2560 14.46 21.5
HSS 5.000×0.500 HSS 127×12.7 5 127 0.5 12.7 0.465 11.8 6.62 4270 24.05 35.8
HSS 5.000×0.375 HSS 127×9.5 5 127 0.375 9.53 0.349 8.86 5.1 3290 18.54 27.6
HSS 5.000×0.312 HSS 127×7.9 5 127 0.312 7.94 0.291 7.39 4.3 2770 15.64 23.3
HSS 5.000×0.258 HSS 127×6.6 5 127 0.258 6.55 0.24 6.1 3.59 2320 13.08 19.5
HSS 5.000×0.250 HSS 127×6.4 5 127 0.25 6.35 0.233 5.92 3.49 2250 12.69 18.9
HSS 5.000×0.188 HSS 127×4.8 5 127 0.188 4.78 0.174 4.42 2.64 1700 9.67 14.4
HSS 5.000×0.125 HSS 127×3.2 5 127 0.125 3.18 0.116 2.95 1.78 1150 6.51 9.69
HSS 4.500×0.375 HSS 114.3×9.5 4.5 114 0.375 9.53 0.349 8.86 4.55 2940 16.54 24.6
HSS 4.500×0.337 HSS 114.3×8.6 4.5 114 0.337 8.56 0.313 7.95 4.12 2660 15 22.3
HSS 4.500×0.237 HSS 114.3×6 4.5 114 0.237 6.02 0.22 5.59 2.96 1910 10.8 16.1
HSS 4.500×0.188 HSS 114.3×4.8 4.5 114 0.188 4.78 0.174 4.42 2.36 1520 8.67 12.9
HSS 4.500×0.125 HSS 114.3×3.2 4.5 114 0.125 3.18 0.116 2.95 1.6 1030 5.85 8.7
HSS 4.000×0.313 HSS 101.6×8 4 102 0.313 7.94 0.291 7.39 3.39 2190 12.34 18.4
HSS 4.000×0.250 HSS 101.6×6.4 4 102 0.25 6.35 0.233 5.92 2.76 1780 10 14.9
HSS 4.000×0.237 HSS 101.6×6 4 102 0.237 6.02 0.22 5.59 2.61 1680 9.53 14.2
HSS 4.000×0.226 HSS 101.6×5.7 4 102 0.226 5.74 0.21 5.33 2.5 1610 9.12 13.6
HSS 4.000×0.220 HSS 101.6×5.6 4 102 0.22 5.59 0.205 5.21 2.44 1570 8.89 13.2
HSS 4.000×0.188 HSS 101.6×4.8 4 102 0.188 4.78 0.174 4.42 2.09 1350 7.66 11.4
HSS 4.000×0.125 HSS 101.6×3.2 4 102 0.125 3.18 0.116 2.95 1.42 916 5.18 7.7
HSS 3.500×0.313 HSS 88.9×8 3.5 88.9 0.313 7.95 0.291 7.39 2.93 1890 10.66 15.9
HSS 3.500×0.300 HSS 88.9×7.6 3.5 88.9 0.3 7.62 0.279 7.09 2.82 1820 10.26 15.3
HSS 3.500×0.250 HSS 88.9×6.4 3.5 88.9 0.25 6.35 0.233 5.92 2.39 1540 8.69 12.9
HSS 3.500×0.216 HSS 88.9×5.5 3.5 88.9 0.216 5.49 0.201 5.11 2.08 1340 7.58 11.3
HSS 3.500×0.203 HSS 88.9×5.2 3.5 88.9 0.203 5.16 0.189 4.8 1.97 1270 7.15 10.6
HSS 3.500×0.188 HSS 88.9×4.8 3.5 88.9 0.188 4.78 0.174 4.42 1.82 1170 6.66 9.9
HSS 3.500×0.125 HSS 88.9×3.2 3.5 88.9 0.125 3.18 0.116 2.95 1.23 794 4.51 6.71
HSS 3.000×0.250 HSS 76.2×6.4 3 76.2 0.25 6.35 0.233 5.92 2.03 1310 7.35 10.9
HSS 3.000×0.216 HSS 76.2×5.5 3 76.2 0.216 5.49 0.201 5.11 1.77 1140 6.43 9.57
HSS 3.000×0.203 HSS 76.2×5.2 3 76.2 0.203 5.16 0.189 4.8 1.67 1080 6.07 9.03
HSS 3.000×0.188 HSS 76.2×4.8 3 76.2 0.188 4.78 0.174 4.42 1.54 994 5.65 8.41
HSS 3.000×0.152 HSS 76.2×3.9 3 76.2 0.152 3.86 0.141 3.58 1.27 819 4.63 6.89
HSS 3.000×0.134 HSS 76.2×3.4 3 76.2 0.134 3.4 0.124 3.15 1.12 723 4.11 6.11
HSS 3.000×0.125 HSS 76.2×3.2 3 76.2 0.125 3.18 0.116 2.95 1.05 677 3.84 5.72
HSS 2.875×0.250 HSS 73×6.4 2.88 73 0.25 6.35 0.233 5.92 1.93 1250 7.02 10.4
HSS 2.875×0.203 HSS 73×5.2 2.88 73 0.203 5.16 0.189 4.8 1.59 1030 5.8 8.63
HSS 2.875×0.188 HSS 73×4.8 2.88 73 0.188 4.78 0.174 4.42 1.48 955 5.4 8.04
HSS 2.875×0.125 HSS 73×3.2 2.88 73 0.125 3.18 0.116 2.95 1.01 652 3.67 5.47
HSS 2.500×0.250 HSS 63.5×6.4 2.5 63.5 0.25 6.35 0.233 5.92 1.66 1070 6.01 8.95
HSS 2.500×0.188 HSS 63.5×4.8 2.5 63.5 0.188 4.78 0.174 4.42 1.27 819 4.65 6.91
HSS 2.500×0.125 HSS 63.5×3.2 2.5 63.5 0.125 3.18 0.116 2.95 0.869 561 3.17 4.72
HSS 2.375×0.250 HSS 60.3×6.4 2.38 60.3 0.25 6.35 0.233 5.92 1.57 1010 5.68 8.45
HSS 2.375×0.218 HSS 60.3×5.5 2.38 60.3 0.218 5.54 0.203 5.16 1.39 897 5.03 7.48
HSS 2.375×0.188 HSS 60.3×4.8 2.38 60.3 0.188 4.78 0.174 4.42 1.2 774 4.4 6.54
HSS 2.375×0.154 HSS 60.3×3.9 2.38 60.3 0.154 3.91 0.143 3.63 1 645 3.66 5.44
HSS 2.375×0.125 HSS 60.3×3.2 2.38 60.3 0.125 3.18 0.116 2.95 0.823 531 3.01 4.47
HSS 1.900×0.188 HSS 48.3×4.8 1.9 48.3 0.188 4.78 0.174 4.42 0.943 608 3.44 5.12
HSS 1.900×0.145 HSS 48.3×3.7 1.9 48.3 0.145 3.68 0.135 3.43 0.749 483 2.72 4.05
HSS 1.900×0.120 HSS 48.3×3.0 1.9 48.3 0.12 3.05 0.111 2.82 0.624 403 2.28 3.4
HSS 1.660×0.140 HSS 42.2×3.6 1.66 42.2 0.14 3.56 0.13 3.3 0.625 403 2.27 3.38

Applications and Service Limits for SA-500-Named Grade B HSS

A500 Grade B HSS is used in building and general structural work within the limits of that ASTM specification and the applicable design standard. Naming the product SA-500 does not add a boiler or pressure-vessel Code listing. Special-shape tubing, coating and any required testing must be stated on the order.

SA-500 Grade B Enquiries Compared with ASTM A500 Grade B, Grade C and A501

The live ASTM Grade B and Grade C pages are ASTM A500 Grade B Steel Hollow Sections (HSS) and ASTM A500 Grade C Steel Hollow Sections (HSS). A Grade C SA-500-named enquiry would need its own companion; this page is Grade B only.

ASTM A501 Grade B is hot-formed tubing with a 65 ksi tensile minimum and a wall-dependent yield. It is not the technical basis of this SA-500 companion.

Near-Equivalents for SA-500 Grade B Enquiries: Not Automatic Substitutes

Near-equivalents only, not automatic substitutes. ASTM A500 Grade B is the technical basis named on this page. ASTM A501, EN 10219 and EN 10210 hollow sections have their own forming routes and mechanical tables. Do not treat a certificate from those specifications as an SA-500 document.

Sourcing SA-500-Named Grade B HSS from SHH STEEL

SHH STEEL reviews the named edition, the Grade B certificate and the ordered HSS designation or outside size and wall before quoting. The typographical AISC HSS table on this page is not a warehouse list.

FAQ: SA-500 Grade B Steel Hollow Sections

Is SA-500 a listed ASME BPVC specification on this page?
No. This companion describes SA-500-named Grade B enquiries on the technical basis of ASTM A500/A500M-23. It does not treat SA-500 as a listed Section II, Part A specification and does not assign an identical-with year.
Does this page replace the ASTM A500 Grade B product page?
No. The ASTM Grade B page remains in place. This is a companion for enquiries that use the SA-500 name. An A500 certificate is not automatically an SA-500 document.
Are these the same sizes as A501?
No. The typographical tables are the AISC Manual 15th Edition HSS subset used on the ASTM A500 Grade B page. They are not A501 hot-formed size tables.

Conclusion

Treat an SA-500 Grade B enquiry as a request that must be compared with ASTM A500/A500M-23 Grade B, not as proof of a listed ASME specification and not as A501. Confirm the edition, Grade B mechanicals and the ordered HSS size before purchase.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X