ASTM A500 Grade B Steel Hollow Sections (HSS)
What are ASTM A500 Grade B Steel Hollow Sections?
ASTM A500 Grade B steel hollow sections are cold-formed carbon steel structural tubing in square, rectangular, round or agreed special shapes, produced welded or seamless to ASTM A500/A500M. The current text used on this page is A500/A500M-23, approved 1 November 2023, which succeeded A500/A500M-21a. The specification covers welded, riveted or bolted construction of bridges and buildings, and general structural purposes, in sizes with a periphery of 88 in [2235 mm] or less and a specified wall thickness of 1.000 in [25.4 mm] or less.
Grade B is the 46 ksi [315 MPa] yield, 58 ksi [400 MPa] tensile grade. Under A500/A500M-23 those minima apply to rounds as well as to squares and rectangles. That matters when someone is still working from a pre-2021 table in which round Grade B was 42 ksi. Grade A no longer appears in the ordering list of the 23 edition (the purchaser specifies Grade B, C or D). Grade D is a 36 ksi grade that requires heat treatment and is not this page.
A500 tubing is not a pressure pipe standard and it is not ASTM A53. It also does not, by itself, specify Charpy V-notch energy. The specification warns that the product may not be suitable where low-temperature notch toughness matters; other ASTM standards exist for those duties. If the enquiry needs a CVN test, a tighter wall tolerance, or a maximum yield, say so on the order rather than assuming Grade B includes them.
Material, Manufacture and Scope for ASTM A500 Grade B HSS
The material is cold-formed carbon steel. Manufacture may be welded (commonly electric-resistance welded from flat-rolled steel) or seamless; the purchase order should name the method if it matters. Shaped tubes (square, rectangular and special) are formed from round or other starting tubes, or formed and welded directly, as the producer’s process allows. Special shapes that are not round, square or rectangular have to be agreed in advance.
Grade, size and the A500/A500M edition belong on the order, together with quantity and length, and with any copper-steel, heat-treatment or testing extras. Dimensional tolerances, straightness, twist, wall and outside-dimension limits are those of the ordered A500/A500M edition. They are not the rolled-shape rules of ASTM A6/A6M, and they are not copied as a second unofficial table here.
ASTM A500 Grade B HSS Sizes: Square, Rectangular and Round (AISC Manual, 15th Edition)
The tables list all 516 hollow structural section designations in the AISC Steel Construction Manual, 15th Edition, shape file (Type = HSS): 107 square (SHS), 281 rectangular (RHS) and 128 round (CHS). Each row joins the inch-pound and SI companion records already used for the live A36 W-shape and S-shape tables. They are reference dimensions for identification and estimating, not a rolling list, and not a claim that every HSS designation is produced, or is currently available, in ASTM A500 Grade B. A500/A500M-23 limits the periphery to 88 in [2235 mm] and the specified wall thickness to 1.000 in [25.4 mm]; every listed designation lies inside those limits (the largest square, HSS 22×22, has a 88 in periphery).
A designation such as HSS 8×8×½ or HSS 20.000×0.375 is a size call: outside dimensions and a specified (nominal) wall. The file also publishes a design wall thickness, tdes, which is about 0.93 of the nominal wall on these rows — the usual AISC practice for electric-resistance-welded A500 HSS. Use the specified wall when ordering and the design wall when the design specification requires it; do not treat the two as interchangeable on the certificate. Corner radii are omitted because a single delivery radius is not published as a unique column in this file, and a radius is not invented here.
Theoretical mass is the tabulated reference value. Settlement should follow the contract — tabulated theoretical mass or weighed mass — and the dimensional tolerances of the ordered A500/A500M edition (not ASTM A6/A6M, which applies to rolled shapes, not to this tubing). These HSS rows are not interchangeable with AISC Pipe designations, with ASTM A53 pipe, or with EN 10219, EN 10210 or GB/T 6728 hollow sections of a similar outside size.
Square HSS (SHS)
107 square designations, grouped by outside size. The first group is the larger squares, from HSS 22×22 down through HSS 10×10.
HSS 22×22 to HSS 10×10
36 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | B (in) | B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 22×22×7/8 | HSS 558.8×558.8×22.2 | 22 | 559 | 0.875 | 22.2 | 0.814 | 20.7 | 67.3 | 43400 | 244.88 | 364 |
| HSS 22×22×3/4 | HSS 558.8×558.8×19 | 22 | 559 | 0.75 | 19.1 | 0.698 | 17.7 | 58.2 | 37600 | 212 | 315 |
| HSS 20×20×7/8 | HSS 508×508×22.2 | 20 | 508 | 0.875 | 22.2 | 0.814 | 20.7 | 60.8 | 39200 | 221.06 | 329 |
| HSS 20×20×3/4 | HSS 508×508×19 | 20 | 508 | 0.75 | 19.1 | 0.698 | 17.7 | 52.6 | 33900 | 191.58 | 285 |
| HSS 20×20×5/8 | HSS 508×508×15.9 | 20 | 508 | 0.625 | 15.9 | 0.581 | 14.8 | 44.3 | 28600 | 161.4 | 240 |
| HSS 20×20×1/2 | HSS 508×508×12.7 | 20 | 508 | 0.5 | 12.7 | 0.465 | 11.8 | 35.8 | 23100 | 130.52 | 194 |
| HSS 18×18×7/8 | HSS 457.2×457.2×22.2 | 18 | 457 | 0.875 | 22.2 | 0.814 | 20.7 | 54.3 | 35000 | 197.24 | 293 |
| HSS 18×18×3/4 | HSS 457.2×457.2×19 | 18 | 457 | 0.75 | 19.1 | 0.698 | 17.7 | 47.1 | 30400 | 171.16 | 255 |
| HSS 18×18×5/8 | HSS 457.2×457.2×15.9 | 18 | 457 | 0.625 | 15.9 | 0.581 | 14.8 | 39.6 | 25500 | 144.39 | 215 |
| HSS 18×18×1/2 | HSS 457.2×457.2×12.7 | 18 | 457 | 0.5 | 12.7 | 0.465 | 11.8 | 32.1 | 20700 | 116.91 | 174 |
| HSS 16×16×7/8 | HSS 406.4×406.4×22.2 | 16 | 406 | 0.875 | 22.2 | 0.814 | 20.7 | 47.7 | 30800 | 173.43 | 258 |
| HSS 16×16×3/4 | HSS 406.4×406.4×19.0 | 16 | 406 | 0.75 | 19.1 | 0.698 | 17.7 | 41.5 | 26800 | 150.75 | 224 |
| HSS 16×16×5/8 | HSS 406.4×406.4×15.9 | 16 | 406 | 0.625 | 15.9 | 0.581 | 14.8 | 35 | 22600 | 127.37 | 189 |
| HSS 16×16×1/2 | HSS 406.4×406.4×12.7 | 16 | 406 | 0.5 | 12.7 | 0.465 | 11.8 | 28.3 | 18300 | 103.3 | 153 |
| HSS 16×16×3/8 | HSS 406.4×406.4×9.5 | 16 | 406 | 0.375 | 9.53 | 0.349 | 8.86 | 21.5 | 13900 | 78.52 | 117 |
| HSS 16×16×5/16 | HSS 406.4×406.4×7.9 | 16 | 406 | 0.3125 | 7.94 | 0.291 | 7.39 | 18.1 | 11700 | 65.87 | 97.9 |
| HSS 14×14×7/8 | HSS 355.6×355.6×22.2 | 14 | 356 | 0.875 | 22.2 | 0.814 | 20.7 | 41.2 | 26600 | 149.61 | 223 |
| HSS 14×14×3/4 | HSS 355.6×355.6×19 | 14 | 356 | 0.75 | 19.1 | 0.698 | 17.7 | 35.9 | 23200 | 130.33 | 194 |
| HSS 14×14×5/8 | HSS 355.6×355.6×15.9 | 14 | 356 | 0.625 | 15.9 | 0.581 | 14.8 | 30.3 | 19500 | 110.36 | 164 |
| HSS 14×14×1/2 | HSS 355.6×355.6×12.7 | 14 | 356 | 0.5 | 12.7 | 0.465 | 11.8 | 24.6 | 15900 | 89.68 | 133 |
| HSS 14×14×3/8 | HSS 355.6×355.6×9.5 | 14 | 356 | 0.375 | 9.53 | 0.349 | 8.86 | 18.7 | 12100 | 68.31 | 102 |
| HSS 14×14×5/16 | HSS 355.6×355.6×7.9 | 14 | 356 | 0.3125 | 7.94 | 0.291 | 7.39 | 15.7 | 10100 | 57.36 | 85.3 |
| HSS 12×12×3/4 | HSS 304.8×304.8×19 | 12 | 305 | 0.75 | 19.1 | 0.698 | 17.7 | 30.3 | 19500 | 109.91 | 164 |
| HSS 12×12×5/8 | HSS 304.8×304.8×15.9 | 12 | 305 | 0.625 | 15.9 | 0.581 | 14.8 | 25.7 | 16600 | 93.34 | 139 |
| HSS 12×12×1/2 | HSS 304.8×304.8×12.7 | 12 | 305 | 0.5 | 12.7 | 0.465 | 11.8 | 20.9 | 13500 | 76.07 | 113 |
| HSS 12×12×3/8 | HSS 304.8×304.8×9.5 | 12 | 305 | 0.375 | 9.53 | 0.349 | 8.86 | 16 | 10300 | 58.1 | 86.3 |
| HSS 12×12×5/16 | HSS 304.8×304.8×7.9 | 12 | 305 | 0.3125 | 7.94 | 0.291 | 7.39 | 13.4 | 8650 | 48.86 | 72.6 |
| HSS 12×12×1/4 | HSS 304.8×304.8×6.4 | 12 | 305 | 0.25 | 6.35 | 0.233 | 5.92 | 10.8 | 6970 | 39.43 | 58.6 |
| HSS 12×12×3/16 | HSS 304.8×304.8×4.8 | 12 | 305 | 0.1875 | 4.76 | 0.174 | 4.42 | 8.15 | 5260 | 29.84 | 44.4 |
| HSS 10×10×3/4 | HSS 254×254×19 | 10 | 254 | 0.75 | 19.1 | 0.698 | 17.7 | 24.7 | 15900 | 89.5 | 133 |
| HSS 10×10×5/8 | HSS 254×254×15.9 | 10 | 254 | 0.625 | 15.9 | 0.581 | 14.8 | 21 | 13500 | 76.33 | 113 |
| HSS 10×10×1/2 | HSS 254×254×12.7 | 10 | 254 | 0.5 | 12.7 | 0.465 | 11.8 | 17.2 | 11100 | 62.46 | 92.7 |
| HSS 10×10×3/8 | HSS 254×254×9.5 | 10 | 254 | 0.375 | 9.53 | 0.349 | 8.86 | 13.2 | 8520 | 47.9 | 71.2 |
| HSS 10×10×5/16 | HSS 254×254×7.9 | 10 | 254 | 0.3125 | 7.94 | 0.291 | 7.39 | 11.1 | 7160 | 40.35 | 60 |
| HSS 10×10×1/4 | HSS 254×254×6.4 | 10 | 254 | 0.25 | 6.35 | 0.233 | 5.92 | 8.96 | 5780 | 32.63 | 48.5 |
| HSS 10×10×3/16 | HSS 254×254×4.8 | 10 | 254 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.76 | 4360 | 24.73 | 36.8 |
HSS 9×9 to HSS 6×6
28 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | B (in) | B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 9×9×5/8 | HSS 228.6×228.6×15.9 | 9 | 229 | 0.625 | 15.9 | 0.581 | 14.8 | 18.7 | 12100 | 67.82 | 101 |
| HSS 9×9×1/2 | HSS 228.6×228.6×12.7 | 9 | 229 | 0.5 | 12.7 | 0.465 | 11.8 | 15.3 | 9870 | 55.66 | 82.6 |
| HSS 9×9×3/8 | HSS 228.6×228.6×9.5 | 9 | 229 | 0.375 | 9.53 | 0.349 | 8.86 | 11.8 | 7610 | 42.79 | 63.6 |
| HSS 9×9×5/16 | HSS 228.6×228.6×7.9 | 9 | 229 | 0.3125 | 7.94 | 0.291 | 7.39 | 9.92 | 6400 | 36.1 | 53.6 |
| HSS 9×9×1/4 | HSS 228.6×228.6×6.4 | 9 | 229 | 0.25 | 6.35 | 0.233 | 5.92 | 8.03 | 5180 | 29.23 | 43.4 |
| HSS 9×9×3/16 | HSS 228.6×228.6×74.8 | 9 | 229 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.06 | 3910 | 22.18 | 33 |
| HSS 9×9×1/8 | HSS 228.6×228.6×3.2 | 9 | 229 | 0.125 | 3.18 | 0.116 | 2.95 | 4.09 | 2640 | 14.96 | 22.3 |
| HSS 8×8×5/8 | HSS 203.2×203.2×15.9 | 8 | 203 | 0.625 | 15.9 | 0.581 | 14.8 | 16.4 | 10600 | 59.32 | 88 |
| HSS 8×8×1/2 | HSS 203.2×203.2×12.7 | 8 | 203 | 0.5 | 12.7 | 0.465 | 11.8 | 13.5 | 8710 | 48.85 | 72.5 |
| HSS 8×8×3/8 | HSS 203.2×203.2×9.5 | 8 | 203 | 0.375 | 9.53 | 0.349 | 8.86 | 10.4 | 6710 | 37.69 | 56 |
| HSS 8×8×5/16 | HSS 203.2×203.2×7.9 | 8 | 203 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.76 | 5650 | 31.84 | 47.3 |
| HSS 8×8×1/4 | HSS 203.2×203.2×6.4 | 8 | 203 | 0.25 | 6.35 | 0.233 | 5.92 | 7.1 | 4580 | 25.82 | 38.4 |
| HSS 8×8×3/16 | HSS 203.2×203.2×4.8 | 8 | 203 | 0.1875 | 4.76 | 0.174 | 4.42 | 5.37 | 3460 | 19.63 | 29.2 |
| HSS 8×8×1/8 | HSS 203.2×203.2×3.2 | 8 | 203 | 0.125 | 3.18 | 0.116 | 2.95 | 3.62 | 2340 | 13.26 | 19.7 |
| HSS 7×7×5/8 | HSS 177.8×177.8×15.9 | 7 | 178 | 0.625 | 15.9 | 0.581 | 14.8 | 14 | 9030 | 50.81 | 75.3 |
| HSS 7×7×1/2 | HSS 177.8×177.8×12.7 | 7 | 178 | 0.5 | 12.7 | 0.465 | 11.8 | 11.6 | 7480 | 42.05 | 62.4 |
| HSS 7×7×3/8 | HSS 177.8×177.8×9.5 | 7 | 178 | 0.375 | 9.53 | 0.349 | 8.86 | 8.97 | 5790 | 32.58 | 48.4 |
| HSS 7×7×5/16 | HSS 177.8×177.8×7.9 | 7 | 178 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.59 | 4900 | 27.59 | 41 |
| HSS 7×7×1/4 | HSS 177.8×177.8×6.4 | 7 | 178 | 0.25 | 6.35 | 0.233 | 5.92 | 6.17 | 3980 | 22.42 | 33.3 |
| HSS 7×7×3/16 | HSS 177.8×177.8×4.8 | 7 | 178 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.67 | 3010 | 17.08 | 25.4 |
| HSS 7×7×1/8 | HSS 177.8×177.8×3.2 | 7 | 178 | 0.125 | 3.18 | 0.116 | 2.95 | 3.16 | 2040 | 11.56 | 17.2 |
| HSS 6×6×5/8 | HSS 152.4×152.4×15.9 | 6 | 152 | 0.625 | 15.9 | 0.581 | 14.8 | 11.7 | 7550 | 42.3 | 62.6 |
| HSS 6×6×1/2 | HSS 152.4×152.4×12.7 | 6 | 152 | 0.5 | 12.7 | 0.465 | 11.8 | 9.74 | 6280 | 35.24 | 52.2 |
| HSS 6×6×3/8 | HSS 152.4×152.4×9.5 | 6 | 152 | 0.375 | 9.53 | 0.349 | 8.86 | 7.58 | 4890 | 27.48 | 40.8 |
| HSS 6×6×5/16 | HSS 152.4×152.4×7.9 | 6 | 152 | 0.3125 | 7.94 | 0.291 | 7.39 | 6.43 | 4150 | 23.34 | 34.6 |
| HSS 6×6×1/4 | HSS 152.4×152.4×6.4 | 6 | 152 | 0.25 | 6.35 | 0.233 | 5.92 | 5.24 | 3380 | 19.02 | 28.3 |
| HSS 6×6×3/16 | HSS 152.4×152.4×4.8 | 6 | 152 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.98 | 2570 | 14.53 | 21.6 |
| HSS 6×6×1/8 | HSS 152.4×152.4×3.2 | 6 | 152 | 0.125 | 3.18 | 0.116 | 2.95 | 2.7 | 1740 | 9.86 | 14.7 |
HSS 5.5×5.5 to HSS 2×2
43 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | B (in) | B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 5-1/2×5-1/2×3/8 | HSS 139.7×139.7×9.5 | 5.5 | 140 | 0.375 | 9.53 | 0.349 | 8.86 | 6.88 | 4440 | 24.93 | 37 |
| HSS 5-1/2×5-1/2×5/16 | HSS 139.7×139.7×7.9 | 5.5 | 140 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.85 | 3770 | 21.21 | 31.5 |
| HSS 5-1/2×5-1/2×1/4 | HSS 139.7×139.7×6.4 | 5.5 | 140 | 0.25 | 6.35 | 0.233 | 5.92 | 4.77 | 3080 | 17.32 | 25.7 |
| HSS 5-1/2×5-1/2×3/16 | HSS 139.7×139.7×4.8 | 5.5 | 140 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.63 | 2340 | 13.25 | 19.7 |
| HSS 5-1/2×5-1/2×1/8 | HSS 139.7×139.7×3.2 | 5.5 | 140 | 0.125 | 3.18 | 0.116 | 2.95 | 2.46 | 1590 | 9.01 | 13.4 |
| HSS 5×5×1/2 | HSS 127×127×12.7 | 5 | 127 | 0.5 | 12.7 | 0.465 | 11.8 | 7.88 | 5080 | 28.43 | 42.1 |
| HSS 5×5×3/8 | HSS 127×127×9.5 | 5 | 127 | 0.375 | 9.53 | 0.349 | 8.86 | 6.18 | 3990 | 22.37 | 33.2 |
| HSS 5×5×5/16 | HSS 127×127×7.9 | 5 | 127 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.26 | 3390 | 19.08 | 28.3 |
| HSS 5×5×1/4 | HSS 127×127×6.4 | 5 | 127 | 0.25 | 6.35 | 0.233 | 5.92 | 4.3 | 2770 | 15.62 | 23.2 |
| HSS 5×5×3/16 | HSS 127×127×4.8 | 5 | 127 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.28 | 2120 | 11.97 | 17.8 |
| HSS 5×5×1/8 | HSS 127×127×3.2 | 5 | 127 | 0.125 | 3.18 | 0.116 | 2.95 | 2.23 | 1440 | 8.16 | 12.1 |
| HSS 4-1/2×4-1/2×1/2 | HSS 114.3×114.3×12.7 | 4.5 | 114 | 0.5 | 12.7 | 0.465 | 11.8 | 6.95 | 4480 | 25.03 | 37.1 |
| HSS 4-1/2×4-1/2×3/8 | HSS 114.3×114.3×9.5 | 4.5 | 114 | 0.375 | 9.53 | 0.349 | 8.86 | 5.48 | 3540 | 19.82 | 29.4 |
| HSS 4-1/2×4-1/2×5/16 | HSS 114.3×114.3×7.9 | 4.5 | 114 | 0.3125 | 7.94 | 0.291 | 7.39 | 4.68 | 3020 | 16.96 | 25.2 |
| HSS 4-1/2×4-1/2×1/4 | HSS 114.3×114.3×6.4 | 4.5 | 114 | 0.25 | 6.35 | 0.233 | 5.92 | 3.84 | 2480 | 13.91 | 20.7 |
| HSS 4-1/2×4-1/2×3/16 | HSS 114.3×114.3×4.8 | 4.5 | 114 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.93 | 1890 | 10.7 | 15.9 |
| HSS 4-1/2×4-1/2×1/8 | HSS 114.3×114.3×3.2 | 4.5 | 114 | 0.125 | 3.18 | 0.116 | 2.95 | 2 | 1290 | 7.31 | 10.9 |
| HSS 4×4×1/2 | HSS 101.6×101.6×12.7 | 4 | 102 | 0.5 | 12.7 | 0.465 | 11.8 | 6.02 | 3880 | 21.63 | 32 |
| HSS 4×4×3/8 | HSS 101.6×101.6×9.5 | 4 | 102 | 0.375 | 9.53 | 0.349 | 8.86 | 4.78 | 3080 | 17.27 | 25.6 |
| HSS 4×4×5/16 | HSS 101.6×101.6×7.9 | 4 | 102 | 0.3125 | 7.94 | 0.291 | 7.39 | 4.1 | 2650 | 14.83 | 22 |
| HSS 4×4×1/4 | HSS 101.6×101.6×6.4 | 4 | 102 | 0.25 | 6.35 | 0.233 | 5.92 | 3.37 | 2170 | 12.21 | 18.1 |
| HSS 4×4×3/16 | HSS 101.6×101.6×4.8 | 4 | 102 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.58 | 1660 | 9.42 | 14 |
| HSS 4×4×1/8 | HSS 101.6×101.6×3.2 | 4 | 102 | 0.125 | 3.18 | 0.116 | 2.95 | 1.77 | 1140 | 6.46 | 9.59 |
| HSS 3-1/2×3-1/2×3/8 | HSS 88.9×88.9×9.5 | 3.5 | 88.9 | 0.375 | 9.53 | 0.349 | 8.86 | 4.09 | 2640 | 14.72 | 21.8 |
| HSS 3-1/2×3-1/2×5/16 | HSS 88.9×88.9×7.9 | 3.5 | 88.9 | 0.3125 | 7.94 | 0.291 | 7.39 | 3.52 | 2270 | 12.7 | 18.8 |
| HSS 3-1/2×3-1/2×1/4 | HSS 88.9×88.9×6.4 | 3.5 | 88.9 | 0.25 | 6.35 | 0.233 | 5.92 | 2.91 | 1880 | 10.51 | 15.6 |
| HSS 3-1/2×3-1/2×3/16 | HSS 88.9×88.9×4.8 | 3.5 | 88.9 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.24 | 1450 | 8.15 | 12.1 |
| HSS 3-1/2×3-1/2×1/8 | HSS 88.9×88.9×3.2 | 3.5 | 88.9 | 0.125 | 3.18 | 0.116 | 2.95 | 1.54 | 994 | 5.61 | 8.33 |
| HSS 3×3×3/8 | HSS 76.2×76.2×9.5 | 3 | 76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 3.39 | 2190 | 12.17 | 18 |
| HSS 3×3×5/16 | HSS 76.2×76.2×7.9 | 3 | 76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 2.94 | 1900 | 10.58 | 15.7 |
| HSS 3×3×1/4 | HSS 76.2×76.2×6.4 | 3 | 76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 2.44 | 1570 | 8.81 | 13.1 |
| HSS 3×3×3/16 | HSS 76.2×76.2×4.8 | 3 | 76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.89 | 1220 | 6.87 | 10.2 |
| HSS 3×3×1/8 | HSS 76.2×76.2×3.2 | 3 | 76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 1.3 | 839 | 4.75 | 7.06 |
| HSS 2-1/2×2-1/2×5/16 | HSS 63.5×63.5×7.9 | 2.5 | 63.5 | 0.3125 | 7.94 | 0.291 | 7.39 | 2.35 | 1520 | 8.45 | 12.5 |
| HSS 2-1/2×2-1/2×1/4 | HSS 63.5×63.5×6.4 | 2.5 | 63.5 | 0.25 | 6.35 | 0.233 | 5.92 | 1.97 | 1270 | 7.11 | 10.5 |
| HSS 2-1/2×2-1/2×3/16 | HSS 63.5×63.5×4.8 | 2.5 | 63.5 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.54 | 994 | 5.59 | 8.3 |
| HSS 2-1/2×2-1/2×1/8 | HSS 63.5×63.5×3.2 | 2.5 | 63.5 | 0.125 | 3.18 | 0.116 | 2.95 | 1.07 | 690 | 3.9 | 5.8 |
| HSS 2-1/4×2-1/4×1/4 | HSS 57.2×57.2×6.4 | 2.25 | 57.2 | 0.25 | 6.35 | 0.233 | 5.92 | 1.74 | 1120 | 6.26 | 9.26 |
| HSS 2-1/4×2-1/4×3/16 | HSS 57.2×57.2×4.8 | 2.25 | 57.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.37 | 884 | 4.96 | 7.35 |
| HSS 2-1/4×2-1/4×1/8 | HSS 57.2×57.2×3.2 | 2.25 | 57.2 | 0.125 | 3.18 | 0.116 | 2.95 | 0.956 | 617 | 3.48 | 5.16 |
| HSS 2×2×1/4 | HSS 50.8×50.8×6.4 | 2 | 50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 1.51 | 974 | 5.41 | 8 |
| HSS 2×2×3/16 | HSS 50.8×50.8×4.8 | 2 | 50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.19 | 768 | 4.32 | 6.4 |
| HSS 2×2×1/8 | HSS 50.8×50.8×3.2 | 2 | 50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 0.84 | 542 | 3.05 | 4.53 |
Rectangular HSS (RHS)
281 rectangular designations, grouped by the longer outside dimension.
HSS 24×… to HSS 16×…
37 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | H×B (in) | H×B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 24×12×3/4 | HSS 609.6×304.8×19 | 24×12 | 610×305 | 0.75 | 19.1 | 0.698 | 17.7 | 47.1 | 30400 | 171.16 | 255 |
| HSS 24×12×5/8 | HSS 609.6×304.8×15.9 | 24×12 | 610×305 | 0.625 | 15.9 | 0.581 | 14.8 | 39.6 | 25500 | 144.39 | 215 |
| HSS 24×12×1/2 | HSS 609.6×304.8×12.7 | 24×12 | 610×305 | 0.5 | 12.7 | 0.465 | 11.8 | 32.1 | 20700 | 116.91 | 174 |
| HSS 20×12×3/4 | HSS 508×304.8×19 | 20×12 | 508×305 | 0.75 | 19.1 | 0.698 | 17.7 | 41.5 | 26800 | 150.75 | 224 |
| HSS 20×12×5/8 | HSS 508×304.8×15.9 | 20×12 | 508×305 | 0.625 | 15.9 | 0.581 | 14.8 | 35 | 22600 | 127.37 | 189 |
| HSS 20×12×1/2 | HSS 508×304.8×12.7 | 20×12 | 508×305 | 0.5 | 12.7 | 0.465 | 11.8 | 28.3 | 18300 | 103.3 | 153 |
| HSS 20×12×3/8 | HSS 508×304.8×9.5 | 20×12 | 508×305 | 0.375 | 9.53 | 0.349 | 8.86 | 21.5 | 13900 | 78.52 | 117 |
| HSS 20×12×5/16 | HSS 508×304.8×7.9 | 20×12 | 508×305 | 0.3125 | 7.94 | 0.291 | 7.39 | 18.1 | 11700 | 65.87 | 97.9 |
| HSS 20×8×5/8 | HSS 508×203.2×15.9 | 20×8 | 508×203 | 0.625 | 15.9 | 0.581 | 14.8 | 30.3 | 19500 | 110.36 | 164 |
| HSS 20×8×1/2 | HSS 508×203.2×12.7 | 20×8 | 508×203 | 0.5 | 12.7 | 0.465 | 11.8 | 24.6 | 15900 | 89.68 | 133 |
| HSS 20×8×3/8 | HSS 508×203.2×9.5 | 20×8 | 508×203 | 0.375 | 9.53 | 0.349 | 8.86 | 18.7 | 12100 | 68.31 | 102 |
| HSS 20×8×5/16 | HSS 508×203.2×7.9 | 20×8 | 508×203 | 0.3125 | 7.94 | 0.291 | 7.39 | 15.7 | 10100 | 57.36 | 85.3 |
| HSS 20×4×1/2 | HSS 508×101.6×12.7 | 20×4 | 508×102 | 0.5 | 12.7 | 0.465 | 11.8 | 20.9 | 13500 | 76.07 | 113 |
| HSS 20×4×3/8 | HSS 508×101.6×9.5 | 20×4 | 508×102 | 0.375 | 9.53 | 0.349 | 8.86 | 16 | 10300 | 58.1 | 86.4 |
| HSS 20×4×5/16 | HSS 508×101.6×7.9 | 20×4 | 508×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 13.4 | 8650 | 48.86 | 72.7 |
| HSS 20×4×1/4 | HSS 508×101.6×6.4 | 20×4 | 508×102 | 0.25 | 6.35 | 0.233 | 5.92 | 10.8 | 6970 | 39.43 | 58.7 |
| HSS 18×6×5/8 | HSS 457.2×152.4×15.9 | 18×6 | 457×152 | 0.625 | 15.9 | 0.581 | 14.8 | 25.7 | 16600 | 93.34 | 139 |
| HSS 18×6×1/2 | HSS 457.2×152.4×12.7 | 18×6 | 457×152 | 0.5 | 12.7 | 0.465 | 11.8 | 20.9 | 13500 | 76.07 | 113 |
| HSS 18×6×3/8 | HSS 457.2×152.4×9.5 | 18×6 | 457×152 | 0.375 | 9.53 | 0.349 | 8.86 | 16 | 10300 | 58.1 | 86.4 |
| HSS 18×6×5/16 | HSS 457.2×152.4×7.9 | 18×6 | 457×152 | 0.3125 | 7.94 | 0.291 | 7.39 | 13.4 | 8650 | 48.86 | 72.7 |
| HSS 18×6×1/4 | HSS 457.2×152.4×6.4 | 18×6 | 457×152 | 0.25 | 6.35 | 0.233 | 5.92 | 10.8 | 6970 | 39.43 | 58.7 |
| HSS 16×12×3/4 | HSS 406.4×304.8×19 | 16×12 | 406×305 | 0.75 | 19.1 | 0.698 | 17.7 | 35.9 | 23200 | 130.33 | 194 |
| HSS 16×12×5/8 | HSS 406.4×304.8×15.9 | 16×12 | 406×305 | 0.625 | 15.9 | 0.581 | 14.8 | 30.3 | 19500 | 110.36 | 164 |
| HSS 16×12×1/2 | HSS 406.4×304.8×12.7 | 16×12 | 406×305 | 0.5 | 12.7 | 0.465 | 11.8 | 24.6 | 15900 | 89.68 | 133 |
| HSS 16×12×3/8 | HSS 406.4×304.8×9.5 | 16×12 | 406×305 | 0.375 | 9.53 | 0.349 | 8.86 | 18.7 | 12100 | 68.31 | 102 |
| HSS 16×12×5/16 | HSS 406.4×304.8×7.9 | 16×12 | 406×305 | 0.3125 | 7.94 | 0.291 | 7.39 | 15.7 | 10100 | 57.36 | 85.4 |
| HSS 16×8×5/8 | HSS 406.4×203.2×15.9 | 16×8 | 406×203 | 0.625 | 15.9 | 0.581 | 14.8 | 25.7 | 16600 | 93.34 | 139 |
| HSS 16×8×1/2 | HSS 406.4×203.2×12.7 | 16×8 | 406×203 | 0.5 | 12.7 | 0.465 | 11.8 | 20.9 | 13500 | 76.07 | 113 |
| HSS 16×8×3/8 | HSS 406.4×203.2×9.5 | 16×8 | 406×203 | 0.375 | 9.53 | 0.349 | 8.86 | 16 | 10300 | 58.1 | 86.4 |
| HSS 16×8×5/16 | HSS 406.4×203.2×7.9 | 16×8 | 406×203 | 0.3125 | 7.94 | 0.291 | 7.39 | 13.4 | 8650 | 48.86 | 72.7 |
| HSS 16×8×1/4 | HSS 406.4×203.2×6.4 | 16×8 | 406×203 | 0.25 | 6.35 | 0.233 | 5.92 | 10.8 | 6970 | 39.43 | 58.7 |
| HSS 16×4×5/8 | HSS 406.4×101.6×15.9 | 16×4 | 406×102 | 0.625 | 15.9 | 0.581 | 14.8 | 21 | 13500 | 76.33 | 113 |
| HSS 16×4×1/2 | HSS 406.4×101.6×12.7 | 16×4 | 406×102 | 0.5 | 12.7 | 0.465 | 11.8 | 17.2 | 11100 | 62.46 | 92.7 |
| HSS 16×4×3/8 | HSS 406.4×101.6×9.5 | 16×4 | 406×102 | 0.375 | 9.53 | 0.349 | 8.86 | 13.2 | 8520 | 47.9 | 71.2 |
| HSS 16×4×5/16 | HSS 406.4×101.6×7.9 | 16×4 | 406×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 11.1 | 7160 | 40.35 | 60 |
| HSS 16×4×1/4 | HSS 406.4×101.6×6.4 | 16×4 | 406×102 | 0.25 | 6.35 | 0.233 | 5.92 | 8.96 | 5780 | 32.63 | 48.6 |
| HSS 16×4×3/16 | HSS 406.4×101.6×4.8 | 16×4 | 406×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.76 | 4360 | 24.73 | 36.7 |
HSS 14×… to HSS 10×…
86 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | H×B (in) | H×B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 14×10×5/8 | HSS 355.6×254×15.9 | 14×10 | 356×254 | 0.625 | 15.9 | 0.581 | 14.8 | 25.7 | 16600 | 93.34 | 139 |
| HSS 14×10×1/2 | HSS 355.6×254×12.7 | 14×10 | 356×254 | 0.5 | 12.7 | 0.465 | 11.8 | 20.9 | 13500 | 76.07 | 113 |
| HSS 14×10×3/8 | HSS 355.6×254×9.5 | 14×10 | 356×254 | 0.375 | 9.53 | 0.349 | 8.86 | 16 | 10300 | 58.1 | 86.4 |
| HSS 14×10×5/16 | HSS 355.6×254×7.9 | 14×10 | 356×254 | 0.3125 | 7.94 | 0.291 | 7.39 | 13.4 | 8650 | 48.86 | 72.7 |
| HSS 14×10×1/4 | HSS 355.6×254×6.4 | 14×10 | 356×254 | 0.25 | 6.35 | 0.233 | 5.92 | 10.8 | 6970 | 39.43 | 58.7 |
| HSS 14×6×5/8 | HSS 355.6×152.4×15.9 | 14×6 | 356×152 | 0.625 | 15.9 | 0.581 | 14.8 | 21 | 13500 | 76.33 | 113 |
| HSS 14×6×1/2 | HSS 355.6×152.4×12.7 | 14×6 | 356×152 | 0.5 | 12.7 | 0.465 | 11.8 | 17.2 | 11100 | 62.46 | 92.7 |
| HSS 14×6×3/8 | HSS 355.6×152.4×9.5 | 14×6 | 356×152 | 0.375 | 9.53 | 0.349 | 8.86 | 13.2 | 8520 | 47.9 | 71.2 |
| HSS 14×6×5/16 | HSS 355.6×152.4×7.9 | 14×6 | 356×152 | 0.3125 | 7.94 | 0.291 | 7.39 | 11.1 | 7160 | 40.35 | 60 |
| HSS 14×6×1/4 | HSS 355.6×152.4×6.4 | 14×6 | 356×152 | 0.25 | 6.35 | 0.233 | 5.92 | 8.96 | 5780 | 32.63 | 48.6 |
| HSS 14×6×3/16 | HSS 355.6×152.4×4.8 | 14×6 | 356×152 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.76 | 4360 | 24.73 | 36.7 |
| HSS 14×4×5/8 | HSS 355.6×101.6×15.9 | 14×4 | 356×102 | 0.625 | 15.9 | 0.581 | 14.8 | 18.7 | 12100 | 67.82 | 101 |
| HSS 14×4×1/2 | HSS 355.6×101.6×12.7 | 14×4 | 356×102 | 0.5 | 12.7 | 0.465 | 11.8 | 15.3 | 9870 | 55.66 | 82.6 |
| HSS 14×4×3/8 | HSS 355.6×101.6×9.5 | 14×4 | 356×102 | 0.375 | 9.53 | 0.349 | 8.86 | 11.8 | 7610 | 42.79 | 63.6 |
| HSS 14×4×5/16 | HSS 355.6×101.6×7.9 | 14×4 | 356×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 9.92 | 6400 | 36.1 | 53.7 |
| HSS 14×4×1/4 | HSS 355.6×101.6×6.4 | 14×4 | 356×102 | 0.25 | 6.35 | 0.233 | 5.92 | 8.03 | 5180 | 29.23 | 43.5 |
| HSS 14×4×3/16 | HSS 355.6×101.6×4.8 | 14×4 | 356×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.06 | 3910 | 22.18 | 32.9 |
| HSS 12×10×1/2 | HSS 304.8×254×12.7 | 12×10 | 305×254 | 0.5 | 12.7 | 0.465 | 11.8 | 19 | 12300 | 69.27 | 103 |
| HSS 12×10×3/8 | HSS 304.8×254×9.5 | 12×10 | 305×254 | 0.375 | 9.53 | 0.349 | 8.86 | 14.6 | 9420 | 53 | 78.8 |
| HSS 12×10×5/16 | HSS 304.8×254×7.9 | 12×10 | 305×254 | 0.3125 | 7.94 | 0.291 | 7.39 | 12.2 | 7870 | 44.6 | 66.4 |
| HSS 12×10×1/4 | HSS 304.8×254×6.4 | 12×10 | 305×254 | 0.25 | 6.35 | 0.233 | 5.92 | 9.9 | 6390 | 36.03 | 53.6 |
| HSS 12×8×5/8 | HSS 304.8×203.2×15.9 | 12×8 | 305×203 | 0.625 | 15.9 | 0.581 | 14.8 | 21 | 13500 | 76.33 | 113 |
| HSS 12×8×1/2 | HSS 304.8×203.2×12.7 | 12×8 | 305×203 | 0.5 | 12.7 | 0.465 | 11.8 | 17.2 | 11100 | 62.46 | 92.7 |
| HSS 12×8×3/8 | HSS 304.8×203.2×9.5 | 12×8 | 305×203 | 0.375 | 9.53 | 0.349 | 8.86 | 13.2 | 8520 | 47.9 | 71.2 |
| HSS 12×8×5/16 | HSS 304.8×203.2×7.9 | 12×8 | 305×203 | 0.3125 | 7.94 | 0.291 | 7.39 | 11.1 | 7160 | 40.35 | 60.1 |
| HSS 12×8×1/4 | HSS 304.8×203.2×6.4 | 12×8 | 305×203 | 0.25 | 6.35 | 0.233 | 5.92 | 8.96 | 5780 | 32.63 | 48.5 |
| HSS 12×8×3/16 | HSS 304.8×203.2×4.8 | 12×8 | 305×203 | 0.1875 | 4.77 | 0.174 | 4.42 | 6.76 | 4360 | 24.73 | 36.9 |
| HSS 12×6×5/8 | HSS 304.8×152.4×15.9 | 12×6 | 305×152 | 0.625 | 15.9 | 0.581 | 14.8 | 18.7 | 12100 | 67.82 | 101 |
| HSS 12×6×1/2 | HSS 304.8×152.4×12.7 | 12×6 | 305×152 | 0.5 | 12.7 | 0.465 | 11.8 | 15.3 | 9870 | 55.66 | 82.6 |
| HSS 12×6×3/8 | HSS 304.8×152.4×9.5 | 12×6 | 305×152 | 0.375 | 9.53 | 0.349 | 8.86 | 11.8 | 7610 | 42.79 | 63.6 |
| HSS 12×6×5/16 | HSS 304.8×152.4×7.9 | 12×6 | 305×152 | 0.3125 | 7.94 | 0.291 | 7.39 | 9.92 | 6400 | 36.1 | 53.7 |
| HSS 12×6×1/4 | HSS 304.8×152.4×6.4 | 12×6 | 305×152 | 0.25 | 6.35 | 0.233 | 5.92 | 8.03 | 5180 | 29.23 | 43.4 |
| HSS 12×6×3/16 | HSS 304.8×152.4×4.8 | 12×6 | 305×152 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.06 | 3910 | 22.18 | 33.1 |
| HSS 12×4×5/8 | HSS 304.8×101.6×15.9 | 12×4 | 305×102 | 0.625 | 15.9 | 0.581 | 14.8 | 16.4 | 10600 | 59.32 | 88 |
| HSS 12×4×1/2 | HSS 304.8×101.6×12.7 | 12×4 | 305×102 | 0.5 | 12.7 | 0.465 | 11.8 | 13.5 | 8710 | 48.85 | 72.5 |
| HSS 12×4×3/8 | HSS 304.8×101.6×9.5 | 12×4 | 305×102 | 0.375 | 9.53 | 0.349 | 8.86 | 10.4 | 6710 | 37.69 | 56 |
| HSS 12×4×5/16 | HSS 304.8×101.6×7.9 | 12×4 | 305×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.76 | 5650 | 31.84 | 47.4 |
| HSS 12×4×1/4 | HSS 304.8×101.6×6.4 | 12×4 | 305×102 | 0.25 | 6.35 | 0.233 | 5.92 | 7.1 | 4580 | 25.82 | 38.4 |
| HSS 12×4×3/16 | HSS 304.8×101.6×4.8 | 12×4 | 305×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 5.37 | 3460 | 19.63 | 29.3 |
| HSS 12×3-1/2×3/8 | HSS 304.8×88.9×9.5 | 12×3.5 | 305×88.9 | 0.375 | 9.53 | 0.349 | 8.86 | 10 | 6450 | 36.41 | 54.1 |
| HSS 12×3-1/2×5/16 | HSS 304.8×88.9×7.9 | 12×3.5 | 305×88.9 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.46 | 5460 | 30.78 | 45.8 |
| HSS 12×3×5/16 | HSS 304.8×76.2×7.9 | 12×3 | 305×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.17 | 5270 | 29.72 | 44.2 |
| HSS 12×3×1/4 | HSS 304.8×76.2×6.4 | 12×3 | 305×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 6.63 | 4280 | 24.12 | 35.8 |
| HSS 12×3×3/16 | HSS 304.8×76.2×4.8 | 12×3 | 305×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 5.02 | 3240 | 18.35 | 27.4 |
| HSS 12×2×5/16 | HSS 304.8×50.8×7.9 | 12×2 | 305×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.59 | 4900 | 27.59 | 41 |
| HSS 12×2×1/4 | HSS 304.8×50.8×6.4 | 12×2 | 305×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 6.17 | 3980 | 22.42 | 33.3 |
| HSS 12×2×3/16 | HSS 304.8×50.8×4.8 | 12×2 | 305×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.67 | 3010 | 17.08 | 25.4 |
| HSS 10×8×5/8 | HSS 254×203.2×15.9 | 10×8 | 254×203 | 0.625 | 15.9 | 0.581 | 14.8 | 18.7 | 12100 | 67.82 | 101 |
| HSS 10×8×1/2 | HSS 254×203.2×12.7 | 10×8 | 254×203 | 0.5 | 12.7 | 0.465 | 11.8 | 15.3 | 9870 | 55.66 | 82.6 |
| HSS 10×8×3/8 | HSS 254×203.2×9.5 | 10×8 | 254×203 | 0.375 | 9.53 | 0.349 | 8.86 | 11.8 | 7610 | 42.79 | 63.6 |
| HSS 10×8×5/16 | HSS 254×203.2×7.9 | 10×8 | 254×203 | 0.3125 | 7.94 | 0.291 | 7.39 | 9.92 | 6400 | 36.1 | 53.7 |
| HSS 10×8×1/4 | HSS 254×203.2×6.4 | 10×8 | 254×203 | 0.25 | 6.35 | 0.233 | 5.92 | 8.03 | 5180 | 29.23 | 43.4 |
| HSS 10×8×3/16 | HSS 254×203.2×4.8 | 10×8 | 254×203 | 0.1875 | 4.76 | 0.174 | 4.42 | 6.06 | 3910 | 22.18 | 33.1 |
| HSS 10×6×5/8 | HSS 254×152.4×15.9 | 10×6 | 254×152 | 0.625 | 15.9 | 0.581 | 14.8 | 16.4 | 10600 | 59.32 | 88 |
| HSS 10×6×1/2 | HSS 254×152.4×12.7 | 10×6 | 254×152 | 0.5 | 12.7 | 0.465 | 11.8 | 13.5 | 8710 | 48.85 | 72.5 |
| HSS 10×6×3/8 | HSS 254×152.4×9.5 | 10×6 | 254×152 | 0.375 | 9.53 | 0.349 | 8.86 | 10.4 | 6710 | 37.69 | 56 |
| HSS 10×6×5/16 | HSS 254×152.4×7.9 | 10×6 | 254×152 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.76 | 5650 | 31.84 | 47.4 |
| HSS 10×6×1/4 | HSS 254×152.4×6.4 | 10×6 | 254×152 | 0.25 | 6.35 | 0.233 | 5.92 | 7.1 | 4580 | 25.82 | 38.4 |
| HSS 10×6×3/16 | HSS 254×152.4×4.8 | 10×6 | 254×152 | 0.1875 | 4.76 | 0.174 | 4.42 | 5.37 | 3460 | 19.63 | 29.3 |
| HSS 10×5×3/8 | HSS 254×127×9.5 | 10×5 | 254×127 | 0.375 | 9.53 | 0.349 | 8.86 | 9.67 | 6240 | 35.13 | 52.2 |
| HSS 10×5×5/16 | HSS 254×127×7.9 | 10×5 | 254×127 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.17 | 5270 | 29.72 | 44.2 |
| HSS 10×5×1/4 | HSS 254×127×6.4 | 10×5 | 254×127 | 0.25 | 6.35 | 0.233 | 5.92 | 6.63 | 4280 | 24.12 | 35.8 |
| HSS 10×5×3/16 | HSS 254×127×4.8 | 10×5 | 254×127 | 0.1875 | 4.76 | 0.174 | 4.42 | 5.02 | 3240 | 18.35 | 27.4 |
| HSS 10×4×5/8 | HSS 254×101.6×15.9 | 10×4 | 254×102 | 0.625 | 15.9 | 0.581 | 14.8 | 14 | 9030 | 50.81 | 75.3 |
| HSS 10×4×1/2 | HSS 254×101.6×12.7 | 10×4 | 254×102 | 0.5 | 12.7 | 0.465 | 11.8 | 11.6 | 7480 | 42.05 | 62.4 |
| HSS 10×4×3/8 | HSS 254×101.6×9.5 | 10×4 | 254×102 | 0.375 | 9.53 | 0.349 | 8.86 | 8.97 | 5790 | 32.58 | 48.4 |
| HSS 10×4×5/16 | HSS 254×101.6×7.9 | 10×4 | 254×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.59 | 4900 | 27.59 | 41 |
| HSS 10×4×1/4 | HSS 254×101.6×6.4 | 10×4 | 254×102 | 0.25 | 6.35 | 0.233 | 5.92 | 6.17 | 3980 | 22.42 | 33.3 |
| HSS 10×4×3/16 | HSS 254×101.6×4.8 | 10×4 | 254×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.67 | 3010 | 17.08 | 25.4 |
| HSS 10×4×1/8 | HSS 254×101.6×3.2 | 10×4 | 254×102 | 0.125 | 3.18 | 0.116 | 2.95 | 3.16 | 2040 | 11.56 | 17.2 |
| HSS 10×3-1/2×1/2 | HSS 254×88.9×12.7 | 10×3.5 | 254×88.9 | 0.5 | 12.7 | 0.465 | 11.8 | 11.1 | 7160 | 40.34 | 59.8 |
| HSS 10×3-1/2×3/8 | HSS 254×88.9×9.5 | 10×3.5 | 254×88.9 | 0.375 | 9.53 | 0.349 | 8.86 | 8.62 | 5560 | 31.31 | 46.5 |
| HSS 10×3-1/2×5/16 | HSS 254×88.9×7.9 | 10×3.5 | 254×88.9 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.3 | 4710 | 26.53 | 39.5 |
| HSS 10×3-1/2×1/4 | HSS 254×88.9×6.4 | 10×3.5 | 254×88.9 | 0.25 | 6.35 | 0.233 | 5.92 | 5.93 | 3830 | 21.57 | 32 |
| HSS 10×3-1/2×3/16 | HSS 254×88.9×4.8 | 10×3.5 | 254×88.9 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.5 | 2900 | 16.44 | 24.5 |
| HSS 10×3-1/2×1/8 | HSS 254×88.9×3.2 | 10×3.5 | 254×88.9 | 0.125 | 3.18 | 0.116 | 2.95 | 3.04 | 1960 | 11.13 | 16.6 |
| HSS 10×3×3/8 | HSS 254×76.2×9.5 | 10×3 | 254×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 8.27 | 5340 | 30.03 | 44.6 |
| HSS 10×3×5/16 | HSS 254×76.2×7.9 | 10×3 | 254×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.01 | 4520 | 25.46 | 37.9 |
| HSS 10×3×1/4 | HSS 254×76.2×6.4 | 10×3 | 254×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 5.7 | 3680 | 20.72 | 30.8 |
| HSS 10×3×3/16 | HSS 254×76.2×4.8 | 10×3 | 254×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.32 | 2790 | 15.8 | 23.5 |
| HSS 10×3×1/8 | HSS 254×76.2×3.2 | 10×3 | 254×76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 2.93 | 1890 | 10.71 | 15.9 |
| HSS 10×2×3/8 | HSS 254×50.8×9.5 | 10×2 | 254×50.8 | 0.375 | 9.53 | 0.349 | 8.86 | 7.58 | 4890 | 27.48 | 40.8 |
| HSS 10×2×5/16 | HSS 254×50.8×7.9 | 10×2 | 254×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 6.43 | 4150 | 23.34 | 34.7 |
| HSS 10×2×1/4 | HSS 254×50.8×6.4 | 10×2 | 254×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 5.24 | 3380 | 19.02 | 28.3 |
| HSS 10×2×3/16 | HSS 254×50.8×4.8 | 10×2 | 254×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.98 | 2570 | 14.53 | 21.6 |
| HSS 10×2×1/8 | HSS 254×50.8×3.2 | 10×2 | 254×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 2.7 | 1740 | 9.86 | 14.7 |
HSS 9×… to HSS 7×…
62 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | H×B (in) | H×B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 9×7×5/8 | HSS 228.6×177.8×15.9 | 9×7 | 229×178 | 0.625 | 15.9 | 0.581 | 14.8 | 16.4 | 10600 | 59.32 | 88 |
| HSS 9×7×1/2 | HSS 228.6×177.8×12.7 | 9×7 | 229×178 | 0.5 | 12.7 | 0.465 | 11.8 | 13.5 | 8710 | 48.85 | 72.5 |
| HSS 9×7×3/8 | HSS 228.6×177.8×9.5 | 9×7 | 229×178 | 0.375 | 9.53 | 0.349 | 8.86 | 10.4 | 6710 | 37.69 | 56 |
| HSS 9×7×5/16 | HSS 228.6×177.8×7.9 | 9×7 | 229×178 | 0.3125 | 7.94 | 0.291 | 7.39 | 8.76 | 5650 | 31.84 | 47.4 |
| HSS 9×7×1/4 | HSS 228.6×177.8×6.4 | 9×7 | 229×178 | 0.25 | 6.35 | 0.233 | 5.92 | 7.1 | 4580 | 25.82 | 38.4 |
| HSS 9×7×3/16 | HSS 228.6×177.8×4.8 | 9×7 | 229×178 | 0.1875 | 4.76 | 0.174 | 4.42 | 5.37 | 3460 | 19.63 | 29.3 |
| HSS 9×5×5/8 | HSS 228.6×127×15.9 | 9×5 | 229×127 | 0.625 | 15.9 | 0.581 | 14.8 | 14 | 9030 | 50.81 | 75.3 |
| HSS 9×5×1/2 | HSS 228.6×127×12.7 | 9×5 | 229×127 | 0.5 | 12.7 | 0.465 | 11.8 | 11.6 | 7480 | 42.05 | 62.4 |
| HSS 9×5×3/8 | HSS 228.6×127×9.5 | 9×5 | 229×127 | 0.375 | 9.53 | 0.349 | 8.86 | 8.97 | 5790 | 32.58 | 48.4 |
| HSS 9×5×5/16 | HSS 228.6×127×7.9 | 9×5 | 229×127 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.59 | 4900 | 27.59 | 41 |
| HSS 9×5×1/4 | HSS 228.6×127×6.4 | 9×5 | 229×127 | 0.25 | 6.35 | 0.233 | 5.92 | 6.17 | 3980 | 22.42 | 33.3 |
| HSS 9×5×3/16 | HSS 228.6×127×4.8 | 9×5 | 229×127 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.67 | 3010 | 17.08 | 25.4 |
| HSS 9×3×1/2 | HSS 228.6×76.2×12.7 | 9×3 | 229×76.2 | 0.5 | 12.7 | 0.465 | 11.8 | 9.74 | 6280 | 35.24 | 52.2 |
| HSS 9×3×3/8 | HSS 228.6×76.2×9.5 | 9×3 | 229×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 7.58 | 4890 | 27.48 | 40.8 |
| HSS 9×3×5/16 | HSS 228.6×76.2×7.9 | 9×3 | 229×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 6.43 | 4150 | 23.34 | 34.7 |
| HSS 9×3×1/4 | HSS 228.6×76.2×6.4 | 9×3 | 229×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 5.24 | 3380 | 19.02 | 28.3 |
| HSS 9×3×3/16 | HSS 228.6×76.2×4.8 | 9×3 | 229×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.98 | 2570 | 14.53 | 21.6 |
| HSS 8×6×5/8 | HSS 203.2×152.4×15.9 | 8×6 | 203×152 | 0.625 | 15.9 | 0.581 | 14.8 | 14 | 9030 | 50.81 | 75.3 |
| HSS 8×6×1/2 | HSS 203.2×152.4×12.7 | 8×6 | 203×152 | 0.5 | 12.7 | 0.465 | 11.8 | 11.6 | 7480 | 42.05 | 62.4 |
| HSS 8×6×3/8 | HSS 203.2×152.4×9.5 | 8×6 | 203×152 | 0.375 | 9.53 | 0.349 | 8.86 | 8.97 | 5790 | 32.58 | 48.4 |
| HSS 8×6×5/16 | HSS 203.2×152.4×7.9 | 8×6 | 203×152 | 0.3125 | 7.94 | 0.291 | 7.39 | 7.59 | 4900 | 27.59 | 41 |
| HSS 8×6×1/4 | HSS 203.2×152.4×6.4 | 8×6 | 203×152 | 0.25 | 6.35 | 0.233 | 5.92 | 6.17 | 3980 | 22.42 | 33.3 |
| HSS 8×6×3/16 | HSS 203.2×152.4×4.8 | 8×6 | 203×152 | 0.1875 | 4.76 | 0.174 | 4.42 | 4.67 | 3010 | 17.08 | 25.4 |
| HSS 8×4×5/8 | HSS 203.2×101.6×15.9 | 8×4 | 203×102 | 0.625 | 15.9 | 0.581 | 14.8 | 11.7 | 7550 | 42.3 | 62.6 |
| HSS 8×4×1/2 | HSS 203.2×101.6×12.7 | 8×4 | 203×102 | 0.5 | 12.7 | 0.465 | 11.8 | 9.74 | 6280 | 35.24 | 52.2 |
| HSS 8×4×3/8 | HSS 203.2×101.6×9.5 | 8×4 | 203×102 | 0.375 | 9.53 | 0.349 | 8.86 | 7.58 | 4890 | 27.48 | 40.8 |
| HSS 8×4×5/16 | HSS 203.2×101.6×7.9 | 8×4 | 203×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 6.43 | 4150 | 23.34 | 34.7 |
| HSS 8×4×1/4 | HSS 203.2×101.6×6.4 | 8×4 | 203×102 | 0.25 | 6.35 | 0.233 | 5.92 | 5.24 | 3380 | 19.02 | 28.3 |
| HSS 8×4×3/16 | HSS 203.2×101.6×4.8 | 8×4 | 203×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.98 | 2570 | 14.53 | 21.6 |
| HSS 8×4×1/8 | HSS 203.2×101.6×3.2 | 8×4 | 203×102 | 0.125 | 3.18 | 0.116 | 2.95 | 2.7 | 1740 | 9.86 | 14.7 |
| HSS 8×3×1/2 | HSS 203.2×76.2×12.7 | 8×3 | 203×76.2 | 0.5 | 12.7 | 0.465 | 11.8 | 8.81 | 5680 | 31.84 | 47.2 |
| HSS 8×3×3/8 | HSS 203.2×76.2×9.5 | 8×3 | 203×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 6.88 | 4440 | 24.93 | 37 |
| HSS 8×3×5/16 | HSS 203.2×76.2×7.9 | 8×3 | 203×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.85 | 3770 | 21.21 | 31.5 |
| HSS 8×3×1/4 | HSS 203.2×76.2×6.4 | 8×3 | 203×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 4.77 | 3080 | 17.32 | 25.7 |
| HSS 8×3×3/16 | HSS 203.2×76.2×4.8 | 8×3 | 203×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.63 | 2340 | 13.25 | 19.7 |
| HSS 8×3×1/8 | HSS 203.2×76.2×3.2 | 8×3 | 203×76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 2.46 | 1590 | 9.01 | 13.4 |
| HSS 8×2×3/8 | HSS 203.2×50.8×9.5 | 8×2 | 203×50.8 | 0.375 | 9.53 | 0.349 | 8.86 | 6.18 | 3990 | 22.37 | 33.2 |
| HSS 8×2×5/16 | HSS 203.2×50.8×7.9 | 8×2 | 203×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.26 | 3390 | 19.08 | 28.4 |
| HSS 8×2×1/4 | HSS 203.2×50.8×6.4 | 8×2 | 203×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 4.3 | 2770 | 15.62 | 23.2 |
| HSS 8×2×3/16 | HSS 203.2×50.8×4.8 | 8×2 | 203×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.28 | 2120 | 11.97 | 17.8 |
| HSS 8×2×1/8 | HSS 203.2×50.8×3.2 | 8×2 | 203×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 2.23 | 1440 | 8.16 | 12.1 |
| HSS 7×5×1/2 | HSS 177.8×127×12.7 | 7×5 | 178×127 | 0.5 | 12.7 | 0.465 | 11.8 | 9.74 | 6280 | 35.24 | 52.2 |
| HSS 7×5×3/8 | HSS 177.8×127×9.5 | 7×5 | 178×127 | 0.375 | 9.53 | 0.349 | 8.86 | 7.58 | 4890 | 27.48 | 40.8 |
| HSS 7×5×5/16 | HSS 177.8×127×7.9 | 7×5 | 178×127 | 0.3125 | 7.94 | 0.291 | 7.39 | 6.43 | 4150 | 23.34 | 34.7 |
| HSS 7×5×1/4 | HSS 177.8×127×6.4 | 7×5 | 178×127 | 0.25 | 6.35 | 0.233 | 5.92 | 5.24 | 3380 | 19.02 | 28.3 |
| HSS 7×5×3/16 | HSS 177.8×127×4.8 | 7×5 | 178×127 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.98 | 2570 | 14.53 | 21.6 |
| HSS 7×5×1/8 | HSS 177.8×127×3.2 | 7×5 | 178×127 | 0.125 | 3.18 | 0.116 | 2.95 | 2.7 | 1740 | 9.86 | 14.7 |
| HSS 7×4×1/2 | HSS 177.8×101.6×12.7 | 7×4 | 178×102 | 0.5 | 12.7 | 0.465 | 11.8 | 8.81 | 5680 | 31.84 | 47.2 |
| HSS 7×4×3/8 | HSS 177.8×101.6×9.5 | 7×4 | 178×102 | 0.375 | 9.53 | 0.349 | 8.86 | 6.88 | 4440 | 24.93 | 37 |
| HSS 7×4×5/16 | HSS 177.8×101.6×7.9 | 7×4 | 178×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.85 | 3770 | 21.21 | 31.5 |
| HSS 7×4×1/4 | HSS 177.8×101.6×6.4 | 7×4 | 178×102 | 0.25 | 6.35 | 0.233 | 5.92 | 4.77 | 3080 | 17.32 | 25.7 |
| HSS 7×4×3/16 | HSS 177.8×101.6×4.8 | 7×4 | 178×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.63 | 2340 | 13.25 | 19.7 |
| HSS 7×4×1/8 | HSS 177.8×101.6×3.2 | 7×4 | 178×102 | 0.125 | 3.18 | 0.116 | 2.95 | 2.46 | 1590 | 9.01 | 13.4 |
| HSS 7×3×1/2 | HSS 177.8×76.2×12.7 | 7×3 | 178×76.2 | 0.5 | 12.7 | 0.465 | 11.8 | 7.88 | 5080 | 28.43 | 42.1 |
| HSS 7×3×3/8 | HSS 177.8×76.2×9.5 | 7×3 | 178×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 6.18 | 3990 | 22.37 | 33.2 |
| HSS 7×3×5/16 | HSS 177.8×76.2×7.9 | 7×3 | 178×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.26 | 3390 | 19.08 | 28.4 |
| HSS 7×3×1/4 | HSS 177.8×76.2×6.4 | 7×3 | 178×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 4.3 | 2770 | 15.62 | 23.2 |
| HSS 7×3×3/16 | HSS 177.8×76.2×4.8 | 7×3 | 178×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.28 | 2120 | 11.97 | 17.8 |
| HSS 7×3×1/8 | HSS 177.8×76.2×3.2 | 7×3 | 178×76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 2.23 | 1440 | 8.16 | 12.1 |
| HSS 7×2×1/4 | HSS 177.8×50.8×6.4 | 7×2 | 178×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 3.84 | 2480 | 13.91 | 20.7 |
| HSS 7×2×3/16 | HSS 177.8×50.8×4.8 | 7×2 | 178×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.93 | 1890 | 10.7 | 15.9 |
| HSS 7×2×1/8 | HSS 177.8×50.8×3.2 | 7×2 | 178×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 2 | 1290 | 7.31 | 10.9 |
HSS 6×… to HSS 5×…
43 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | H×B (in) | H×B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 6×5×1/2 | HSS 152.4×127×12.7 | 6×5 | 152×127 | 0.5 | 12.7 | 0.465 | 11.8 | 8.81 | 5680 | 31.84 | 47.2 |
| HSS 6×5×3/8 | HSS 152.4×127×9.5 | 6×5 | 152×127 | 0.375 | 9.53 | 0.349 | 8.86 | 6.88 | 4440 | 24.93 | 37 |
| HSS 6×5×5/16 | HSS 152.4×127×7.9 | 6×5 | 152×127 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.85 | 3770 | 21.21 | 31.5 |
| HSS 6×5×1/4 | HSS 152.4×127×6.4 | 6×5 | 152×127 | 0.25 | 6.35 | 0.233 | 5.92 | 4.77 | 3080 | 17.32 | 25.7 |
| HSS 6×5×3/16 | HSS 152.4×127×4.8 | 6×5 | 152×127 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.63 | 2340 | 13.25 | 19.7 |
| HSS 6×5×1/8 | HSS 152.4×127×3.2 | 6×5 | 152×127 | 0.125 | 3.18 | 0.116 | 2.95 | 2.46 | 1590 | 9.01 | 13.4 |
| HSS 6×4×1/2 | HSS 152.4×101.6×12.7 | 6×4 | 152×102 | 0.5 | 12.7 | 0.465 | 11.8 | 7.88 | 5080 | 28.43 | 42.1 |
| HSS 6×4×3/8 | HSS 152.4×101.6×9.5 | 6×4 | 152×102 | 0.375 | 9.53 | 0.349 | 8.86 | 6.18 | 3990 | 22.37 | 33.2 |
| HSS 6×4×5/16 | HSS 152.4×101.6×7.9 | 6×4 | 152×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 5.26 | 3390 | 19.08 | 28.4 |
| HSS 6×4×1/4 | HSS 152.4×101.6×6.4 | 6×4 | 152×102 | 0.25 | 6.35 | 0.233 | 5.92 | 4.3 | 2770 | 15.62 | 23.2 |
| HSS 6×4×3/16 | HSS 152.4×101.6×4.8 | 6×4 | 152×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 3.28 | 2120 | 11.97 | 17.8 |
| HSS 6×4×1/8 | HSS 152.4×101.6×3.2 | 6×4 | 152×102 | 0.125 | 3.18 | 0.116 | 2.95 | 2.23 | 1440 | 8.16 | 12.1 |
| HSS 6×3×1/2 | HSS 152.4×76.2×12.7 | 6×3 | 152×76.2 | 0.5 | 12.7 | 0.465 | 11.8 | 6.95 | 4480 | 25.03 | 37.1 |
| HSS 6×3×3/8 | HSS 152.4×76.2×9.5 | 6×3 | 152×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 5.48 | 3540 | 19.82 | 29.4 |
| HSS 6×3×5/16 | HSS 152.4×76.2×7.9 | 6×3 | 152×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 4.68 | 3020 | 16.96 | 25.2 |
| HSS 6×3×1/4 | HSS 152.4×76.2×6.4 | 6×3 | 152×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 3.84 | 2480 | 13.91 | 20.7 |
| HSS 6×3×3/16 | HSS 152.4×76.2×4.8 | 6×3 | 152×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.93 | 1890 | 10.7 | 15.9 |
| HSS 6×3×1/8 | HSS 152.4×76.2×3.2 | 6×3 | 152×76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 2 | 1290 | 7.31 | 10.9 |
| HSS 6×2×3/8 | HSS 152.4×50.8×9.5 | 6×2 | 152×50.8 | 0.375 | 9.53 | 0.349 | 8.86 | 4.78 | 3080 | 17.27 | 25.6 |
| HSS 6×2×5/16 | HSS 152.4×50.8×7.9 | 6×2 | 152×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 4.1 | 2650 | 14.83 | 22 |
| HSS 6×2×1/4 | HSS 152.4×50.8×6.4 | 6×2 | 152×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 3.37 | 2170 | 12.21 | 18.1 |
| HSS 6×2×3/16 | HSS 152.4×50.8×4.8 | 6×2 | 152×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.58 | 1660 | 9.42 | 14 |
| HSS 6×2×1/8 | HSS 152.4×50.8×3.2 | 6×2 | 152×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 1.77 | 1140 | 6.46 | 9.59 |
| HSS 5×4×1/2 | HSS 127×101.6×12.7 | 5×4 | 127×102 | 0.5 | 12.7 | 0.465 | 11.8 | 6.95 | 4480 | 25.03 | 37.1 |
| HSS 5×4×3/8 | HSS 127×101.6×9.5 | 5×4 | 127×102 | 0.375 | 9.53 | 0.349 | 8.86 | 5.48 | 3540 | 19.82 | 29.4 |
| HSS 5×4×5/16 | HSS 127×101.6×7.9 | 5×4 | 127×102 | 0.3125 | 7.94 | 0.291 | 7.39 | 4.68 | 3020 | 16.96 | 25.2 |
| HSS 5×4×1/4 | HSS 127×101.6×6.4 | 5×4 | 127×102 | 0.25 | 6.35 | 0.233 | 5.92 | 3.84 | 2480 | 13.91 | 20.7 |
| HSS 5×4×3/16 | HSS 127×101.6×4.8 | 5×4 | 127×102 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.93 | 1890 | 10.7 | 15.9 |
| HSS 5×4×1/8 | HSS 127×101.6×3.2 | 5×4 | 127×102 | 0.125 | 3.18 | 0.116 | 2.95 | 2 | 1290 | 7.31 | 10.9 |
| HSS 5×3×1/2 | HSS 127×76.2×12.7 | 5×3 | 127×76.2 | 0.5 | 12.7 | 0.465 | 11.8 | 6.02 | 3880 | 21.63 | 32 |
| HSS 5×3×3/8 | HSS 127×76.2×9.5 | 5×3 | 127×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 4.78 | 3080 | 17.27 | 25.6 |
| HSS 5×3×5/16 | HSS 127×76.2×7.9 | 5×3 | 127×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 4.1 | 2650 | 14.83 | 22 |
| HSS 5×3×1/4 | HSS 127×76.2×6.4 | 5×3 | 127×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 3.37 | 2170 | 12.21 | 18.1 |
| HSS 5×3×3/16 | HSS 127×76.2×4.8 | 5×3 | 127×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.58 | 1660 | 9.42 | 14 |
| HSS 5×3×1/8 | HSS 127×76.2×3.2 | 5×3 | 127×76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 1.77 | 1140 | 6.46 | 9.59 |
| HSS 5×2-1/2×1/4 | HSS 127×63.5×6.4 | 5×2.5 | 127×63.5 | 0.25 | 6.35 | 0.233 | 5.92 | 3.14 | 2030 | 11.36 | 16.9 |
| HSS 5×2-1/2×3/16 | HSS 127×63.5×4.8 | 5×2.5 | 127×63.5 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.41 | 1550 | 8.78 | 13.1 |
| HSS 5×2-1/2×1/8 | HSS 127×63.5×3.2 | 5×2.5 | 127×63.5 | 0.125 | 3.18 | 0.116 | 2.95 | 1.65 | 1060 | 6.03 | 8.96 |
| HSS 5×2×3/8 | HSS 127×50.8×9.5 | 5×2 | 127×50.8 | 0.375 | 9.53 | 0.349 | 8.86 | 4.09 | 2640 | 14.72 | 21.8 |
| HSS 5×2×5/16 | HSS 127×50.8×7.9 | 5×2 | 127×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 3.52 | 2270 | 12.7 | 18.8 |
| HSS 5×2×1/4 | HSS 127×50.8×6.4 | 5×2 | 127×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 2.91 | 1880 | 10.51 | 15.6 |
| HSS 5×2×3/16 | HSS 127×50.8×4.8 | 5×2 | 127×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.24 | 1450 | 8.15 | 12.1 |
| HSS 5×2×1/8 | HSS 127×50.8×3.2 | 5×2 | 127×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 1.54 | 994 | 5.61 | 8.33 |
HSS 4.5×… to HSS 2×…
53 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | H×B (in) | H×B (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 4×3×3/8 | HSS 101.6×76.2×9.5 | 4×3 | 102×76.2 | 0.375 | 9.53 | 0.349 | 8.86 | 4.09 | 2640 | 14.72 | 21.8 |
| HSS 4×3×5/16 | HSS 101.6×76.2×7.9 | 4×3 | 102×76.2 | 0.3125 | 7.94 | 0.291 | 7.39 | 3.52 | 2270 | 12.7 | 18.8 |
| HSS 4×3×1/4 | HSS 101.6×76.2×6.4 | 4×3 | 102×76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 2.91 | 1880 | 10.51 | 15.6 |
| HSS 4×3×3/16 | HSS 101.6×76.2×4.8 | 4×3 | 102×76.2 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.24 | 1450 | 8.15 | 12.1 |
| HSS 4×3×1/8 | HSS 101.6×76.2×3.2 | 4×3 | 102×76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 1.54 | 994 | 5.61 | 8.33 |
| HSS 4×2-1/2×3/8 | HSS 101.6×63.5×9.5 | 4×2.5 | 102×63.5 | 0.375 | 9.53 | 0.349 | 8.86 | 3.74 | 2410 | 13.44 | 19.9 |
| HSS 4×2-1/2×5/16 | HSS 101.6×63.5×7.9 | 4×2.5 | 102×63.5 | 0.3125 | 7.94 | 0.291 | 7.39 | 3.23 | 2080 | 11.64 | 17.3 |
| HSS 4×2-1/2×1/4 | HSS 101.6×63.5×6.4 | 4×2.5 | 102×63.5 | 0.25 | 6.35 | 0.233 | 5.92 | 2.67 | 1720 | 9.66 | 14.3 |
| HSS 4×2-1/2×3/16 | HSS 101.6×63.5×4.8 | 4×2.5 | 102×63.5 | 0.1875 | 4.76 | 0.174 | 4.42 | 2.06 | 1330 | 7.51 | 11.2 |
| HSS 4×2-1/2×1/8 | HSS 101.6×63.5×3.2 | 4×2.5 | 102×63.5 | 0.125 | 3.18 | 0.116 | 2.95 | 1.42 | 916 | 5.18 | 7.7 |
| HSS 4×2×3/8 | HSS 101.6×50.8×9.5 | 4×2 | 102×50.8 | 0.375 | 9.53 | 0.349 | 8.86 | 3.39 | 2190 | 12.17 | 18 |
| HSS 4×2×5/16 | HSS 101.6×50.8×7.9 | 4×2 | 102×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 2.94 | 1900 | 10.58 | 15.7 |
| HSS 4×2×1/4 | HSS 101.6×50.8×6.4 | 4×2 | 102×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 2.44 | 1570 | 8.81 | 13.1 |
| HSS 4×2×3/16 | HSS 101.6×50.8×4.8 | 4×2 | 102×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.89 | 1220 | 6.87 | 10.2 |
| HSS 4×2×1/8 | HSS 101.6×50.8×3.2 | 4×2 | 102×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 1.3 | 839 | 4.75 | 7.06 |
| HSS 3-1/2×2-1/2×3/8 | HSS 88.9×63.5×9.5 | 3.5×2.5 | 88.9×63.5 | 0.375 | 9.53 | 0.349 | 8.86 | 3.39 | 2190 | 12.17 | 18 |
| HSS 3-1/2×2-1/2×5/16 | HSS 88.9×63.5×7.9 | 3.5×2.5 | 88.9×63.5 | 0.3125 | 7.94 | 0.291 | 7.39 | 2.94 | 1900 | 10.58 | 15.6 |
| HSS 3-1/2×2-1/2×1/4 | HSS 88.9×63.5×6.4 | 3.5×2.5 | 88.9×63.5 | 0.25 | 6.35 | 0.233 | 5.92 | 2.44 | 1570 | 8.81 | 13.1 |
| HSS 3-1/2×2-1/2×3/16 | HSS 88.9×63.5×4.8 | 3.5×2.5 | 88.9×63.5 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.89 | 1220 | 6.87 | 10.2 |
| HSS 3-1/2×2-1/2×1/8 | HSS 88.9×63.5×3.2 | 3.5×2.5 | 88.9×63.5 | 0.125 | 3.18 | 0.116 | 2.95 | 1.3 | 839 | 4.75 | 7.07 |
| HSS 3-1/2×2×1/4 | HSS 88.9×50.8×6.4 | 3.5×2 | 88.9×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 2.21 | 1430 | 7.96 | 11.8 |
| HSS 3-1/2×2×3/16 | HSS 88.9×50.8×4.8 | 3.5×2 | 88.9×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.71 | 1100 | 6.23 | 9.27 |
| HSS 3-1/2×2×1/8 | HSS 88.9×50.8×3.2 | 3.5×2 | 88.9×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 1.19 | 768 | 4.33 | 6.43 |
| HSS 3-1/2×1-1/2×1/4 | HSS 88.9×38.1×6.4 | 3.5×1.5 | 88.9×38.1 | 0.25 | 6.35 | 0.233 | 5.92 | 1.97 | 1270 | 7.11 | 10.5 |
| HSS 3-1/2×1-1/2×3/16 | HSS 88.9×38.1×4.8 | 3.5×1.5 | 88.9×38.1 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.54 | 994 | 5.59 | 8.31 |
| HSS 3-1/2×1-1/2×1/8 | HSS 88.9×38.1×3.2 | 3.5×1.5 | 88.9×38.1 | 0.125 | 3.18 | 0.116 | 2.95 | 1.07 | 690 | 3.9 | 5.8 |
| HSS 3×2-1/2×5/16 | HSS 76.2×63.5×7.9 | 3×2.5 | 76.2×63.5 | 0.3125 | 7.94 | 0.291 | 7.39 | 2.64 | 1700 | 9.51 | 14.1 |
| HSS 3×2-1/2×1/4 | HSS 76.2×63.5×6.4 | 3×2.5 | 76.2×63.5 | 0.25 | 6.35 | 0.233 | 5.92 | 2.21 | 1430 | 7.96 | 11.8 |
| HSS 3×2-1/2×3/16 | HSS 76.2×63.5×4.8 | 3×2.5 | 76.2×63.5 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.71 | 1100 | 6.23 | 9.27 |
| HSS 3×2-1/2×1/8 | HSS 76.2×63.5×3.2 | 3×2.5 | 76.2×63.5 | 0.125 | 3.18 | 0.116 | 2.95 | 1.19 | 768 | 4.33 | 6.43 |
| HSS 3×2×5/16 | HSS 76.2×50.8×7.9 | 3×2 | 76.2×50.8 | 0.3125 | 7.94 | 0.291 | 7.39 | 2.35 | 1520 | 8.45 | 12.5 |
| HSS 3×2×1/4 | HSS 76.2×50.8×6.4 | 3×2 | 76.2×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 1.97 | 1270 | 7.11 | 10.5 |
| HSS 3×2×3/16 | HSS 76.2×50.8×4.8 | 3×2 | 76.2×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.54 | 994 | 5.59 | 8.31 |
| HSS 3×2×1/8 | HSS 76.2×50.8×3.2 | 3×2 | 76.2×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 1.07 | 690 | 3.9 | 5.8 |
| HSS 3×1-1/2×1/4 | HSS 76.2×38.1×6.4 | 3×1.5 | 76.2×38.1 | 0.25 | 6.35 | 0.233 | 5.92 | 1.74 | 1120 | 6.26 | 9.26 |
| HSS 3×1-1/2×3/16 | HSS 76.2×38.1×4.8 | 3×1.5 | 76.2×38.1 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.37 | 884 | 4.96 | 7.36 |
| HSS 3×1-1/2×1/8 | HSS 76.2×38.1×3.2 | 3×1.5 | 76.2×38.1 | 0.125 | 3.18 | 0.116 | 2.95 | 0.956 | 617 | 3.48 | 5.16 |
| HSS 3×1×3/16 | HSS 76.2×25.4×4.8 | 3×1 | 76.2×25.4 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.19 | 768 | 4.32 | 6.41 |
| HSS 3×1×1/8 | HSS 76.2×25.4×3.2 | 3×1 | 76.2×25.4 | 0.125 | 3.18 | 0.116 | 2.95 | 0.84 | 542 | 3.05 | 4.53 |
| HSS 2-1/2×2×1/4 | HSS 63.5×50.8×6.4 | 2.5×2 | 63.5×50.8 | 0.25 | 6.35 | 0.233 | 5.92 | 1.74 | 1120 | 6.26 | 9.26 |
| HSS 2-1/2×2×3/16 | HSS 63.5×50.8×4.8 | 2.5×2 | 63.5×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.37 | 884 | 4.96 | 7.36 |
| HSS 2-1/2×2×1/8 | HSS 63.5×50.8×3.2 | 2.5×2 | 63.5×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 0.956 | 617 | 3.48 | 5.16 |
| HSS 2-1/2×1-1/2×1/4 | HSS 63.5×38.1×6.4 | 2.5×1.5 | 63.5×38.1 | 0.25 | 6.35 | 0.233 | 5.92 | 1.51 | 974 | 5.41 | 8 |
| HSS 2-1/2×1-1/2×3/16 | HSS 63.5×38.1×4.8 | 2.5×1.5 | 63.5×38.1 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.19 | 768 | 4.32 | 6.41 |
| HSS 2-1/2×1-1/2×1/8 | HSS 63.5×38.1×3.2 | 2.5×1.5 | 63.5×38.1 | 0.125 | 3.18 | 0.116 | 2.95 | 0.84 | 542 | 3.05 | 4.53 |
| HSS 2-1/2×1×3/16 | HSS 63.5×25.4×4.8 | 2.5×1 | 63.5×25.4 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.02 | 658 | 3.68 | 5.46 |
| HSS 2-1/2×1×1/8 | HSS 63.5×25.4×3.2 | 2.5×1 | 63.5×25.4 | 0.125 | 3.18 | 0.116 | 2.95 | 0.724 | 467 | 2.63 | 3.9 |
| HSS 2-1/4×2×3/16 | HSS 57.2×50.8×4.8 | 2.25×2 | 57.2×50.8 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.28 | 826 | 4.64 | 6.89 |
| HSS 2-1/4×2×1/8 | HSS 57.2×50.8×3.2 | 2.25×2 | 57.2×50.8 | 0.125 | 3.18 | 0.116 | 2.95 | 0.898 | 579 | 3.27 | 4.85 |
| HSS 2×1-1/2×3/16 | HSS 50.8×38.1×4.8 | 2×1.5 | 50.8×38.1 | 0.1875 | 4.76 | 0.174 | 4.42 | 1.02 | 658 | 3.68 | 5.46 |
| HSS 2×1-1/2×1/8 | HSS 50.8×38.1×3.2 | 2×1.5 | 50.8×38.1 | 0.125 | 3.18 | 0.116 | 2.95 | 0.724 | 467 | 2.63 | 3.9 |
| HSS 2×1×3/16 | HSS 50.8×25.4×4.8 | 2×1 | 50.8×25.4 | 0.1875 | 4.76 | 0.174 | 4.42 | 0.845 | 545 | 3.04 | 4.51 |
| HSS 2×1×1/8 | HSS 50.8×25.4×3.2 | 2×1 | 50.8×25.4 | 0.125 | 3.18 | 0.116 | 2.95 | 0.608 | 392 | 2.2 | 3.26 |
Round HSS (CHS)
128 round designations, grouped by outside diameter. These are HSS, not AISC Pipe and not ASTM A53 pipe, even when the outside diameter looks familiar.
HSS 20.000 to HSS 10.000
27 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | OD (in) | OD (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 20.000×0.500 | HSS 508×12.7 | 20 | 508 | 0.5 | 12.7 | 0.465 | 11.8 | 28.5 | 18400 | 104 | 155 |
| HSS 20.000×0.375 | HSS 508×9.5 | 20 | 508 | 0.375 | 9.53 | 0.349 | 8.86 | 21.5 | 13900 | 78.67 | 117 |
| HSS 18.000×0.500 | HSS 457.2×12.7 | 18 | 457 | 0.5 | 12.7 | 0.465 | 11.8 | 25.6 | 16500 | 93.54 | 139 |
| HSS 18.000×0.375 | HSS 457.2×9.5 | 18 | 457 | 0.375 | 9.53 | 0.349 | 8.86 | 19.4 | 12500 | 70.66 | 105 |
| HSS 16.000×0.625 | HSS 406.4×15.9 | 16 | 406 | 0.625 | 15.9 | 0.581 | 14.8 | 28.1 | 18100 | 103 | 153 |
| HSS 16.000×0.500 | HSS 406.4×12.7 | 16 | 406 | 0.5 | 12.7 | 0.465 | 11.8 | 22.7 | 14600 | 82.85 | 123 |
| HSS 16.000×0.438 | HSS 406.4×11.1 | 16 | 406 | 0.438 | 11.1 | 0.407 | 10.3 | 19.9 | 12800 | 72.87 | 108 |
| HSS 16.000×0.375 | HSS 406.4×9.5 | 16 | 406 | 0.375 | 9.53 | 0.349 | 8.86 | 17.2 | 11100 | 62.64 | 93.2 |
| HSS 16.000×0.312 | HSS 406.4×7.9 | 16 | 406 | 0.312 | 7.94 | 0.291 | 7.39 | 14.4 | 9290 | 52.32 | 77.9 |
| HSS 16.000×0.250 | HSS 406.4×6.4 | 16 | 406 | 0.25 | 6.35 | 0.233 | 5.92 | 11.5 | 7420 | 42.09 | 62.6 |
| HSS 14.000×0.625 | HSS 355.6×15.9 | 14 | 356 | 0.625 | 15.9 | 0.581 | 14.8 | 24.5 | 15800 | 89.36 | 133 |
| HSS 14.000×0.500 | HSS 355.6×12.7 | 14 | 356 | 0.5 | 12.7 | 0.465 | 11.8 | 19.8 | 12800 | 72.16 | 107 |
| HSS 14.000×0.375 | HSS 355.6×9.5 | 14 | 356 | 0.375 | 9.53 | 0.349 | 8.86 | 15 | 9680 | 54.62 | 81.3 |
| HSS 14.000×0.312 | HSS 355.6×7.9 | 14 | 356 | 0.312 | 7.94 | 0.291 | 7.39 | 12.5 | 8060 | 45.65 | 67.9 |
| HSS 14.000×0.250 | HSS 355.6×6.4 | 14 | 356 | 0.25 | 6.35 | 0.233 | 5.92 | 10.1 | 6520 | 36.75 | 54.7 |
| HSS 12.750×0.500 | HSS 323.9×12.7 | 12.8 | 324 | 0.5 | 12.7 | 0.465 | 11.8 | 17.9 | 11500 | 65.48 | 97.4 |
| HSS 12.750×0.375 | HSS 323.9×9.5 | 12.8 | 324 | 0.375 | 9.53 | 0.349 | 8.86 | 13.6 | 8770 | 49.61 | 73.8 |
| HSS 12.750×0.250 | HSS 323.9×6.4 | 12.8 | 324 | 0.25 | 6.35 | 0.233 | 5.92 | 9.16 | 5910 | 33.41 | 49.7 |
| HSS 10.750×0.500 | HSS 273.1×12.7 | 10.8 | 273 | 0.5 | 12.7 | 0.465 | 11.8 | 15 | 9680 | 54.79 | 81.5 |
| HSS 10.750×0.375 | HSS 273.1×9.5 | 10.8 | 273 | 0.375 | 9.53 | 0.349 | 8.86 | 11.4 | 7350 | 41.59 | 61.9 |
| HSS 10.750×0.250 | HSS 273.1×6.4 | 10.8 | 273 | 0.25 | 6.35 | 0.233 | 5.92 | 7.7 | 4970 | 28.06 | 41.8 |
| HSS 10.000×0.625 | HSS 254×15.9 | 10 | 254 | 0.625 | 15.9 | 0.581 | 14.8 | 17.2 | 11100 | 62.64 | 93.2 |
| HSS 10.000×0.500 | HSS 254×12.7 | 10 | 254 | 0.5 | 12.7 | 0.465 | 11.8 | 13.9 | 8970 | 50.78 | 75.6 |
| HSS 10.000×0.375 | HSS 254×9.5 | 10 | 254 | 0.375 | 9.53 | 0.349 | 8.86 | 10.6 | 6840 | 38.58 | 57.4 |
| HSS 10.000×0.312 | HSS 254×7.9 | 10 | 254 | 0.312 | 7.94 | 0.291 | 7.39 | 8.88 | 5730 | 32.31 | 48.1 |
| HSS 10.000×0.250 | HSS 254×6.4 | 10 | 254 | 0.25 | 6.35 | 0.233 | 5.92 | 7.15 | 4610 | 26.06 | 38.8 |
| HSS 10.000×0.188 | HSS 254×4.8 | 10 | 254 | 0.188 | 4.78 | 0.174 | 4.42 | 5.37 | 3460 | 19.72 | 29.3 |
HSS 9.625 to HSS 5.563
49 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | OD (in) | OD (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 9.625×0.500 | HSS 244.5×12.7 | 9.63 | 244 | 0.5 | 12.7 | 0.465 | 11.8 | 13.4 | 8650 | 48.77 | 72.6 |
| HSS 9.625×0.375 | HSS 244.5×9.5 | 9.63 | 244 | 0.375 | 9.53 | 0.349 | 8.86 | 10.2 | 6580 | 37.08 | 55.2 |
| HSS 9.625×0.312 | HSS 244.5×7.9 | 9.63 | 244 | 0.312 | 7.94 | 0.291 | 7.39 | 8.53 | 5500 | 31.06 | 46.2 |
| HSS 9.625×0.250 | HSS 244.5×6.4 | 9.63 | 244 | 0.25 | 6.35 | 0.233 | 5.92 | 6.87 | 4430 | 25.06 | 37.3 |
| HSS 9.625×0.188 | HSS 244.5×4.8 | 9.63 | 244 | 0.188 | 4.78 | 0.174 | 4.42 | 5.17 | 3340 | 18.97 | 28.2 |
| HSS 8.625×0.625 | HSS 219.1×15.9 | 8.63 | 219 | 0.625 | 15.9 | 0.581 | 14.8 | 14.7 | 9480 | 53.45 | 79.5 |
| HSS 8.625×0.500 | HSS 219.1×12.7 | 8.63 | 219 | 0.5 | 12.7 | 0.465 | 11.8 | 11.9 | 7680 | 43.43 | 64.6 |
| HSS 8.625×0.375 | HSS 219.1×9.5 | 8.63 | 219 | 0.375 | 9.53 | 0.349 | 8.86 | 9.07 | 5850 | 33.07 | 49.2 |
| HSS 8.625×0.322 | HSS 219.1×8.2 | 8.63 | 219 | 0.322 | 8.18 | 0.3 | 7.62 | 7.85 | 5060 | 28.58 | 42.5 |
| HSS 8.625×0.250 | HSS 219.1×6.4 | 8.63 | 219 | 0.25 | 6.35 | 0.233 | 5.92 | 6.14 | 3960 | 22.38 | 33.3 |
| HSS 8.625×0.188 | HSS 219.1×4.8 | 8.63 | 219 | 0.188 | 4.78 | 0.174 | 4.42 | 4.62 | 2980 | 16.96 | 25.2 |
| HSS 7.625×0.375 | HSS 193.7×9.5 | 7.63 | 194 | 0.375 | 9.53 | 0.349 | 8.86 | 7.98 | 5150 | 29.06 | 43.2 |
| HSS 7.625×0.328 | HSS 193.7×8.3 | 7.63 | 194 | 0.328 | 8.33 | 0.305 | 7.75 | 7.01 | 4520 | 25.59 | 38.1 |
| HSS 7.500×0.500 | HSS 190.5×12.7 | 7.5 | 191 | 0.5 | 12.7 | 0.465 | 11.8 | 10.3 | 6650 | 37.42 | 55.7 |
| HSS 7.500×0.375 | HSS 190.5×9.5 | 7.5 | 191 | 0.375 | 9.53 | 0.349 | 8.86 | 7.84 | 5060 | 28.56 | 42.5 |
| HSS 7.500×0.312 | HSS 190.5×7.9 | 7.5 | 191 | 0.312 | 7.94 | 0.291 | 7.39 | 6.59 | 4250 | 23.97 | 35.7 |
| HSS 7.500×0.250 | HSS 190.5×6.4 | 7.5 | 191 | 0.25 | 6.35 | 0.233 | 5.92 | 5.32 | 3430 | 19.38 | 28.8 |
| HSS 7.500×0.188 | HSS 190.5×4.8 | 7.5 | 191 | 0.188 | 4.78 | 0.174 | 4.42 | 4 | 2580 | 14.7 | 21.9 |
| HSS 7.000×0.500 | HSS 177.8×12.7 | 7 | 178 | 0.5 | 12.7 | 0.465 | 11.8 | 9.55 | 6160 | 34.74 | 51.7 |
| HSS 7.000×0.375 | HSS 177.8×9.5 | 7 | 178 | 0.375 | 9.53 | 0.349 | 8.86 | 7.29 | 4700 | 26.56 | 39.5 |
| HSS 7.000×0.312 | HSS 177.8×7.9 | 7 | 178 | 0.312 | 7.94 | 0.291 | 7.39 | 6.13 | 3950 | 22.31 | 33.2 |
| HSS 7.000×0.250 | HSS 177.8×6.4 | 7 | 178 | 0.25 | 6.35 | 0.233 | 5.92 | 4.95 | 3190 | 18.04 | 26.8 |
| HSS 7.000×0.188 | HSS 177.8×4.8 | 7 | 178 | 0.188 | 4.78 | 0.174 | 4.42 | 3.73 | 2410 | 13.69 | 20.4 |
| HSS 7.000×0.125 | HSS 177.8×3.2 | 7 | 178 | 0.125 | 3.18 | 0.116 | 2.95 | 2.51 | 1620 | 9.19 | 13.7 |
| HSS 6.875×0.500 | HSS 174.6×12.7 | 6.88 | 175 | 0.5 | 12.7 | 0.465 | 11.8 | 9.36 | 6040 | 34.07 | 50.7 |
| HSS 6.875×0.375 | HSS 174.6×9.5 | 6.88 | 175 | 0.375 | 9.53 | 0.349 | 8.86 | 7.16 | 4620 | 26.06 | 38.8 |
| HSS 6.875×0.312 | HSS 174.6×7.9 | 6.88 | 175 | 0.312 | 7.94 | 0.291 | 7.39 | 6.02 | 3880 | 21.89 | 32.6 |
| HSS 6.875×0.250 | HSS 174.6×6.4 | 6.88 | 175 | 0.25 | 6.35 | 0.233 | 5.92 | 4.86 | 3140 | 17.71 | 26.3 |
| HSS 6.875×0.188 | HSS 174.6×4.8 | 6.88 | 175 | 0.188 | 4.78 | 0.174 | 4.42 | 3.66 | 2360 | 13.44 | 20 |
| HSS 6.625×0.500 | HSS 168.3×12.7 | 6.63 | 168 | 0.5 | 12.7 | 0.465 | 11.8 | 9 | 5810 | 32.74 | 48.7 |
| HSS 6.625×0.432 | HSS 168.3×11 | 6.63 | 168 | 0.432 | 11.1 | 0.402 | 10.2 | 7.86 | 5070 | 28.6 | 42.6 |
| HSS 6.625×0.375 | HSS 168.3×9.5 | 6.63 | 168 | 0.375 | 9.53 | 0.349 | 8.86 | 6.88 | 4440 | 25.06 | 37.3 |
| HSS 6.625×0.312 | HSS 168.3×7.9 | 6.63 | 168 | 0.312 | 7.94 | 0.291 | 7.39 | 5.79 | 3740 | 21.06 | 31.3 |
| HSS 6.625×0.280 | HSS 168.3×7.1 | 6.63 | 168 | 0.28 | 7.11 | 0.26 | 6.6 | 5.2 | 3350 | 18.99 | 28.3 |
| HSS 6.625×0.250 | HSS 168.3×6.4 | 6.63 | 168 | 0.25 | 6.35 | 0.233 | 5.92 | 4.68 | 3020 | 17.04 | 25.4 |
| HSS 6.625×0.188 | HSS 168.3×4.8 | 6.63 | 168 | 0.188 | 4.78 | 0.174 | 4.42 | 3.53 | 2280 | 12.94 | 19.2 |
| HSS 6.625×0.125 | HSS 168.3×3.2 | 6.63 | 168 | 0.125 | 3.18 | 0.116 | 2.95 | 2.37 | 1530 | 8.69 | 12.9 |
| HSS 6.000×0.500 | HSS 152.4×12.7 | 6 | 152 | 0.5 | 12.7 | 0.465 | 11.8 | 8.09 | 5220 | 29.4 | 43.7 |
| HSS 6.000×0.375 | HSS 152.4×9.5 | 6 | 152 | 0.375 | 9.53 | 0.349 | 8.86 | 6.2 | 4000 | 22.55 | 33.6 |
| HSS 6.000×0.312 | HSS 152.4×7.9 | 6 | 152 | 0.312 | 7.94 | 0.291 | 7.39 | 5.22 | 3370 | 18.97 | 28.2 |
| HSS 6.000×0.280 | HSS 152.4×7.1 | 6 | 152 | 0.28 | 7.11 | 0.26 | 6.6 | 4.69 | 3030 | 17.12 | 25.5 |
| HSS 6.000×0.250 | HSS 152.4×6.4 | 6 | 152 | 0.25 | 6.35 | 0.233 | 5.92 | 4.22 | 2720 | 15.37 | 22.9 |
| HSS 6.000×0.188 | HSS 152.4×4.8 | 6 | 152 | 0.188 | 4.78 | 0.174 | 4.42 | 3.18 | 2050 | 11.68 | 17.4 |
| HSS 6.000×0.125 | HSS 152.4×3.2 | 6 | 152 | 0.125 | 3.18 | 0.116 | 2.95 | 2.14 | 1380 | 7.85 | 11.7 |
| HSS 5.563×0.500 | HSS 141.3×12.7 | 5.56 | 141 | 0.5 | 12.7 | 0.465 | 11.8 | 7.45 | 4810 | 27.06 | 40.3 |
| HSS 5.563×0.375 | HSS 141.3×9.5 | 5.56 | 141 | 0.375 | 9.53 | 0.349 | 8.86 | 5.72 | 3690 | 20.8 | 30.9 |
| HSS 5.563×0.258 | HSS 141.3×6.6 | 5.56 | 141 | 0.258 | 6.55 | 0.24 | 6.1 | 4.01 | 2590 | 14.63 | 21.8 |
| HSS 5.563×0.188 | HSS 141.3×4.8 | 5.56 | 141 | 0.188 | 4.78 | 0.174 | 4.42 | 2.95 | 1900 | 10.8 | 16.1 |
| HSS 5.563×0.134 | HSS 141.3×3.4 | 5.56 | 141 | 0.134 | 3.4 | 0.124 | 3.15 | 2.12 | 1370 | 7.78 | 11.6 |
HSS 5.000 to HSS 1.660
52 designations in this group.
Swipe horizontally to view all dimensions.
| Designation | SI designation | OD (in) | OD (mm) | tnom (in) | tnom (mm) | tdes (in) | tdes (mm) | A (in²) | A (mm²) | Mass (lb/ft) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| HSS 5.500×0.500 | HSS 139.7×12.7 | 5.5 | 140 | 0.5 | 12.7 | 0.465 | 11.8 | 7.36 | 4750 | 26.73 | 39.8 |
| HSS 5.500×0.375 | HSS 139.7×9.5 | 5.5 | 140 | 0.375 | 9.53 | 0.349 | 8.86 | 5.65 | 3650 | 20.55 | 30.6 |
| HSS 5.500×0.258 | HSS 139.7×6.6 | 5.5 | 140 | 0.258 | 6.55 | 0.24 | 6.1 | 3.97 | 2560 | 14.46 | 21.5 |
| HSS 5.000×0.500 | HSS 127×12.7 | 5 | 127 | 0.5 | 12.7 | 0.465 | 11.8 | 6.62 | 4270 | 24.05 | 35.8 |
| HSS 5.000×0.375 | HSS 127×9.5 | 5 | 127 | 0.375 | 9.53 | 0.349 | 8.86 | 5.1 | 3290 | 18.54 | 27.6 |
| HSS 5.000×0.312 | HSS 127×7.9 | 5 | 127 | 0.312 | 7.94 | 0.291 | 7.39 | 4.3 | 2770 | 15.64 | 23.3 |
| HSS 5.000×0.258 | HSS 127×6.6 | 5 | 127 | 0.258 | 6.55 | 0.24 | 6.1 | 3.59 | 2320 | 13.08 | 19.5 |
| HSS 5.000×0.250 | HSS 127×6.4 | 5 | 127 | 0.25 | 6.35 | 0.233 | 5.92 | 3.49 | 2250 | 12.69 | 18.9 |
| HSS 5.000×0.188 | HSS 127×4.8 | 5 | 127 | 0.188 | 4.78 | 0.174 | 4.42 | 2.64 | 1700 | 9.67 | 14.4 |
| HSS 5.000×0.125 | HSS 127×3.2 | 5 | 127 | 0.125 | 3.18 | 0.116 | 2.95 | 1.78 | 1150 | 6.51 | 9.69 |
| HSS 4.500×0.375 | HSS 114.3×9.5 | 4.5 | 114 | 0.375 | 9.53 | 0.349 | 8.86 | 4.55 | 2940 | 16.54 | 24.6 |
| HSS 4.500×0.337 | HSS 114.3×8.6 | 4.5 | 114 | 0.337 | 8.56 | 0.313 | 7.95 | 4.12 | 2660 | 15 | 22.3 |
| HSS 4.500×0.237 | HSS 114.3×6 | 4.5 | 114 | 0.237 | 6.02 | 0.22 | 5.59 | 2.96 | 1910 | 10.8 | 16.1 |
| HSS 4.500×0.188 | HSS 114.3×4.8 | 4.5 | 114 | 0.188 | 4.78 | 0.174 | 4.42 | 2.36 | 1520 | 8.67 | 12.9 |
| HSS 4.500×0.125 | HSS 114.3×3.2 | 4.5 | 114 | 0.125 | 3.18 | 0.116 | 2.95 | 1.6 | 1030 | 5.85 | 8.7 |
| HSS 4.000×0.313 | HSS 101.6×8 | 4 | 102 | 0.313 | 7.94 | 0.291 | 7.39 | 3.39 | 2190 | 12.34 | 18.4 |
| HSS 4.000×0.250 | HSS 101.6×6.4 | 4 | 102 | 0.25 | 6.35 | 0.233 | 5.92 | 2.76 | 1780 | 10 | 14.9 |
| HSS 4.000×0.237 | HSS 101.6×6 | 4 | 102 | 0.237 | 6.02 | 0.22 | 5.59 | 2.61 | 1680 | 9.53 | 14.2 |
| HSS 4.000×0.226 | HSS 101.6×5.7 | 4 | 102 | 0.226 | 5.74 | 0.21 | 5.33 | 2.5 | 1610 | 9.12 | 13.6 |
| HSS 4.000×0.220 | HSS 101.6×5.6 | 4 | 102 | 0.22 | 5.59 | 0.205 | 5.21 | 2.44 | 1570 | 8.89 | 13.2 |
| HSS 4.000×0.188 | HSS 101.6×4.8 | 4 | 102 | 0.188 | 4.78 | 0.174 | 4.42 | 2.09 | 1350 | 7.66 | 11.4 |
| HSS 4.000×0.125 | HSS 101.6×3.2 | 4 | 102 | 0.125 | 3.18 | 0.116 | 2.95 | 1.42 | 916 | 5.18 | 7.7 |
| HSS 3.500×0.313 | HSS 88.9×8 | 3.5 | 88.9 | 0.313 | 7.95 | 0.291 | 7.39 | 2.93 | 1890 | 10.66 | 15.9 |
| HSS 3.500×0.300 | HSS 88.9×7.6 | 3.5 | 88.9 | 0.3 | 7.62 | 0.279 | 7.09 | 2.82 | 1820 | 10.26 | 15.3 |
| HSS 3.500×0.250 | HSS 88.9×6.4 | 3.5 | 88.9 | 0.25 | 6.35 | 0.233 | 5.92 | 2.39 | 1540 | 8.69 | 12.9 |
| HSS 3.500×0.216 | HSS 88.9×5.5 | 3.5 | 88.9 | 0.216 | 5.49 | 0.201 | 5.11 | 2.08 | 1340 | 7.58 | 11.3 |
| HSS 3.500×0.203 | HSS 88.9×5.2 | 3.5 | 88.9 | 0.203 | 5.16 | 0.189 | 4.8 | 1.97 | 1270 | 7.15 | 10.6 |
| HSS 3.500×0.188 | HSS 88.9×4.8 | 3.5 | 88.9 | 0.188 | 4.78 | 0.174 | 4.42 | 1.82 | 1170 | 6.66 | 9.9 |
| HSS 3.500×0.125 | HSS 88.9×3.2 | 3.5 | 88.9 | 0.125 | 3.18 | 0.116 | 2.95 | 1.23 | 794 | 4.51 | 6.71 |
| HSS 3.000×0.250 | HSS 76.2×6.4 | 3 | 76.2 | 0.25 | 6.35 | 0.233 | 5.92 | 2.03 | 1310 | 7.35 | 10.9 |
| HSS 3.000×0.216 | HSS 76.2×5.5 | 3 | 76.2 | 0.216 | 5.49 | 0.201 | 5.11 | 1.77 | 1140 | 6.43 | 9.57 |
| HSS 3.000×0.203 | HSS 76.2×5.2 | 3 | 76.2 | 0.203 | 5.16 | 0.189 | 4.8 | 1.67 | 1080 | 6.07 | 9.03 |
| HSS 3.000×0.188 | HSS 76.2×4.8 | 3 | 76.2 | 0.188 | 4.78 | 0.174 | 4.42 | 1.54 | 994 | 5.65 | 8.41 |
| HSS 3.000×0.152 | HSS 76.2×3.9 | 3 | 76.2 | 0.152 | 3.86 | 0.141 | 3.58 | 1.27 | 819 | 4.63 | 6.89 |
| HSS 3.000×0.134 | HSS 76.2×3.4 | 3 | 76.2 | 0.134 | 3.4 | 0.124 | 3.15 | 1.12 | 723 | 4.11 | 6.11 |
| HSS 3.000×0.125 | HSS 76.2×3.2 | 3 | 76.2 | 0.125 | 3.18 | 0.116 | 2.95 | 1.05 | 677 | 3.84 | 5.72 |
| HSS 2.875×0.250 | HSS 73×6.4 | 2.88 | 73 | 0.25 | 6.35 | 0.233 | 5.92 | 1.93 | 1250 | 7.02 | 10.4 |
| HSS 2.875×0.203 | HSS 73×5.2 | 2.88 | 73 | 0.203 | 5.16 | 0.189 | 4.8 | 1.59 | 1030 | 5.8 | 8.63 |
| HSS 2.875×0.188 | HSS 73×4.8 | 2.88 | 73 | 0.188 | 4.78 | 0.174 | 4.42 | 1.48 | 955 | 5.4 | 8.04 |
| HSS 2.875×0.125 | HSS 73×3.2 | 2.88 | 73 | 0.125 | 3.18 | 0.116 | 2.95 | 1.01 | 652 | 3.67 | 5.47 |
| HSS 2.500×0.250 | HSS 63.5×6.4 | 2.5 | 63.5 | 0.25 | 6.35 | 0.233 | 5.92 | 1.66 | 1070 | 6.01 | 8.95 |
| HSS 2.500×0.188 | HSS 63.5×4.8 | 2.5 | 63.5 | 0.188 | 4.78 | 0.174 | 4.42 | 1.27 | 819 | 4.65 | 6.91 |
| HSS 2.500×0.125 | HSS 63.5×3.2 | 2.5 | 63.5 | 0.125 | 3.18 | 0.116 | 2.95 | 0.869 | 561 | 3.17 | 4.72 |
| HSS 2.375×0.250 | HSS 60.3×6.4 | 2.38 | 60.3 | 0.25 | 6.35 | 0.233 | 5.92 | 1.57 | 1010 | 5.68 | 8.45 |
| HSS 2.375×0.218 | HSS 60.3×5.5 | 2.38 | 60.3 | 0.218 | 5.54 | 0.203 | 5.16 | 1.39 | 897 | 5.03 | 7.48 |
| HSS 2.375×0.188 | HSS 60.3×4.8 | 2.38 | 60.3 | 0.188 | 4.78 | 0.174 | 4.42 | 1.2 | 774 | 4.4 | 6.54 |
| HSS 2.375×0.154 | HSS 60.3×3.9 | 2.38 | 60.3 | 0.154 | 3.91 | 0.143 | 3.63 | 1 | 645 | 3.66 | 5.44 |
| HSS 2.375×0.125 | HSS 60.3×3.2 | 2.38 | 60.3 | 0.125 | 3.18 | 0.116 | 2.95 | 0.823 | 531 | 3.01 | 4.47 |
| HSS 1.900×0.188 | HSS 48.3×4.8 | 1.9 | 48.3 | 0.188 | 4.78 | 0.174 | 4.42 | 0.943 | 608 | 3.44 | 5.12 |
| HSS 1.900×0.145 | HSS 48.3×3.7 | 1.9 | 48.3 | 0.145 | 3.68 | 0.135 | 3.43 | 0.749 | 483 | 2.72 | 4.05 |
| HSS 1.900×0.120 | HSS 48.3×3.0 | 1.9 | 48.3 | 0.12 | 3.05 | 0.111 | 2.82 | 0.624 | 403 | 2.28 | 3.4 |
| HSS 1.660×0.140 | HSS 42.2×3.6 | 1.66 | 42.2 | 0.14 | 3.56 | 0.13 | 3.3 | 0.625 | 403 | 2.27 | 3.38 |
ASTM A500 Grade B Chemical Composition (Heat and Product Analysis)
Heat and product analysis limits below are the Grade B (and Grade D) columns of ASTM A500/A500M-23 Table 1. Grade C is a tighter carbon maximum and is tabulated on the Grade C page; do not apply the Grade C carbon limit to a Grade B-only certificate, or the other way around. Values are mass percent.
ASTM A500/A500M-23 chemical requirements for Grades B and D.
Swipe horizontally to view all dimensions.
| Element | Heat analysis | Product analysis |
|---|---|---|
| Carbon, maxA | 0.26 | 0.30 |
| Manganese, maxA | 1.35 | 1.40 |
| Phosphorus, max | 0.035 | 0.045 |
| Sulfur, max | 0.035 | 0.045 |
| Copper, minB | 0.20 | 0.18 |
A For each reduction of 0.01 percentage point below the specified carbon maximum, an increase of 0.06 percentage point above the specified manganese maximum is permitted, up to 1.50 % by heat analysis and 1.60 % by product analysis.
B Copper minimum applies only if copper-containing steel is specified in the purchase order.
ASTM A500 Grade B Mechanical Properties: Yield, Tensile and Elongation
From ASTM A500/A500M-23 Table 2, the Grade B tensile requirements apply to round, square, rectangular and special tubular shapes alike. That is a change from earlier editions, in which round Grade B had a 42 ksi [290 MPa] yield minimum and only the shaped product was 46 ksi. If the order names A500/A500M-23 (or A500/A500M-21 / 21a, which already unified the shapes), do not design or certify Grade B rounds to the obsolete 42 ksi figure. An older certificate must be read against the edition actually printed on it.
Swipe horizontally to view all dimensions.
| Property | Grade B (all shapes) |
|---|---|
| Tensile strength, min, psi [MPa] | 58 000 [400] |
| Yield strength, min, psi [MPa] | 46 000 [315] |
| Elongation in 2 in [50 mm], min, % | 23 |
The 23 % elongation in 2 in [50 mm] applies to specified wall thicknesses of 0.180 in [4.57 mm] and greater. For lighter specified walls the minimum is 61t + 12, rounded to the nearest percent (t in inches). For A500M the matching formula is 2.4t + 12, with t in millimetres. Specified elongation applies to tests performed before shipment.
Delivery, Inspection and Identification of ASTM A500 Grade B HSS
Grade B does not require the heat treatment that Grade D requires. Delivery condition is the as-cold-formed welded or seamless product, unless the order adds a treatment. Identification and inspection should allow the tube to be traced to a mill certificate that names ASTM A500/A500M, the edition, Grade B, the size (outside dimensions and specified wall), and whether the product is welded or seamless. A certificate that only says “A500” or only “HSS”, without the grade, is not a Grade B document.
Round tubing is subject to the flattening (or agreed alternative) tests of the ordered edition. Those production tests are not a substitute for a project-specified Charpy test, which A500 does not impose by default.
Weldability and Surface Condition of ASTM A500 Grade B HSS
Grade B is a carbon steel in the ordinary structural range and is routinely welded, provided the procedure matches the thickness, the manufacturing method (welded or seamless) and any coating. The as-formed surface and the weld seam of an ERW tube are part of the product; do not assume a ground-flush seam or a shot-blasted finish unless the order says so. If the member is a dynamically loaded, welded element that needs verified toughness, Grade B by itself is not that specification.
Dimensional Tolerances and Theoretical Mass for ASTM A500 Grade B HSS
Outside dimensions, wall thickness, length, straightness, squareness and twist are accepted to the tolerances in the ordered A500/A500M edition. Those rules are different from ASTM A6/A6M (rolled W, S and C shapes) and from ASTM A53 (pipe). They are also different from the tighter wall and tighter mass practice in ASTM A1085, which is a separate HSS specification and is not a silent upgrade of Grade B.
On the AISC rows tabulated here, the design wall tdes is about 0.93 of the specified wall. Design calculations that use tdes must still procure the matching specified wall. Theoretical masses in the tables are AISC reference values, not a weighed-mass guarantee.
Applications and Service Limits for ASTM A500 Grade B Steel Hollow Sections
Grade B HSS is widely used for building frames, trusses, columns, bracing, conveyor supports and general fabricated structures where a 46 ksi yield is the design basis and a Charpy test is not required. It is not, without extras, a low-temperature toughness grade, a pressure-vessel pipe, or a weathering grade. It is also not a hot-finished hollow section: ASTM A501 and EN 10210 are different products, with different residual-stress and corner-radius expectations.
Where the design already assumes 50 ksi, Grade C — or a dual Grade B and Grade C certificate that actually meets Grade C — is the matching callout, not a hope that Grade B will “come in high”.
ASTM A500 Grade B Compared with Grade C, A1085, A501 and EN 10219
Grade C in A500/A500M-23 is 50 ksi [345 MPa] yield and 62 ksi [425 MPa] tensile for the same family of shapes. Many producers issue dual Grade B and Grade C certificates; that document can support a Grade B callout only if Grade B is actually named and met, and it can support a Grade C callout only if Grade C is actually met. A Grade B-only certificate does not satisfy a Grade C specification.
ASTM A1085 is a later HSS specification with a different tolerance and property package (including a documented maximum yield in the current practice of that standard) and is not an automatic substitute for A500 Grade B. ASTM A501 covers hot-formed tubing. EN 10219-1 cold-formed hollow sections and EN 10210-1 hot-finished hollow sections are European delivery standards; an S235JRH or S355J2H certificate is not an A500 Grade B certificate, and the geometric series are not the AISC HSS list. ASME SA-500 is only relevant when the order actually requires the ASME mark; it is not implied by an ASTM A500 Grade B line.
Near-Equivalents for ASTM A500 Grade B HSS: Not Automatic Substitutes
Engineers sometimes compare Grade B with EN 10219-1 S275 or S235 families, or with GB/T 6728 Q235B, because the yield bands sit in a similar neighbourhood. Those comparisons are starting points for a substitution study, not a licence to restamp the tube. Chemistry, elongation wall-thickness rules, impact testing, tolerances, corner radii and the design-wall convention all differ. Any substitution has to be accepted by the purchaser against the edition named on the order.
Grade C, A1085, A501, A53 and SA-500 are neighbouring ASTM or ASME products, not equivalents of Grade B.
Sourcing ASTM A500 Grade B Steel Hollow Sections from SHH STEEL
SHH STEEL reviews enquiries for ASTM A500 Grade B HSS against the grade letter, the A500/A500M edition, the outside size and specified wall, welded or seamless manufacture, and the certificate that will accompany the tubes. The 516-row table is a reference list, not a catalogue of guaranteed mill items. Lengths, surface condition and any additional tests (including Charpy, if required) should be written on the enquiry so they can be checked before a quotation is prepared.
ASTM A500 Grade B HSS FAQs
-
Is ASTM A500 Grade B still 42 ksi for round HSS?
- Not under A500/A500M-21, 21a or 23. Those editions set 46 ksi [315 MPa] minimum yield for rounds as well as for squares and rectangles. The 42 ksi round figure belongs to earlier editions and should only be used when the certificate actually names one of those earlier editions.
-
Are all 516 AISC HSS sizes stocked in Grade B?
- No. The tables are the complete AISC Manual, 15th Edition, HSS list used as a reference. They are not a claim that every designation is produced, or held, in Grade B. Size, wall and length are confirmed against the enquiry.
-
Is a dual Grade B and Grade C certificate acceptable for a Grade B order?
- It can be, when the certificate actually names Grade B (or both grades) and the tests meet Grade B. A Grade C-only certificate is not automatically Grade B, and a Grade B-only certificate is not Grade C.
-
Is A500 Grade B the same as ASTM A53 or AISC Pipe?
- No. A500 is structural tubing. A53 and the AISC Pipe designations are pipe products with different scopes, tests and tolerances. A round HSS and a Pipe of similar outside diameter are not interchangeable on the paperwork.
-
Does Grade B include a Charpy test?
- Not by default. A500/A500M notes that the product may not be suitable where low-temperature notch toughness is important. If a CVN test is required, it has to be specified on the order.
Conclusion
ASTM A500 Grade B HSS is the 46 ksi [315 MPa] / 58 ksi [400 MPa] cold-formed carbon steel hollow section of A500/A500M-23, covering square, rectangular and round tubing within the 88 in periphery and 1.000 in wall envelope. The size tables reprint the 516 AISC Manual, 15th Edition, HSS designations as a reference, not as a stock list. Confirm the edition, the grade letter, the specified wall and the certificate before the tubes are released to the job.