JIS G4401 SK105 Tool Steel Plate | JIS G4401 Tool Steel - SHH STEEL

JIS G4401 SK105 Tool Steel Plate

JIS G 4401 SK105 is a high-carbon water-hardening tool steel plate with a heat-analysis carbon range of 1.00–1.10 %. Typical tools include hacksaws, chisels, gauges, springs, press dies, jigs and cutting tools that need a hard, wear-resistant edge after hardening. Plate is ordinarily supplied as-hot-rolled; annealed or cold-rolled plate may be agreed when a softer condition is needed for machining. SHH STEEL produces and exports SK105 plate to the ordered edition, condition and dimensions.
Equivalent Grades:
ISO 4957 C105U (JIS G 4401:2009 Annex JB, near name). Previously referenced as SK3.
Heat Treatment
As-hot-rolled; annealed or cold-rolled by agreement (JIS G 4401:2009).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is JIS G 4401 SK105 plate?

We produce and export JIS G 4401 SK105 as carbon tool steel plate. SK105 is a water-hardening carbon tool steel with a heat-analysis carbon range of 1.00–1.10 %. Typical tools include hacksaws, chisels, gauges, springs, press dies, jigs and cutting tools. Wear resistance after hardening rises, and toughness falls, as carbon increases through the JIS G 4401 series.

Composition and hardness values on this page follow JIS G 4401:2009. Specify the edition required on the purchase order.

SHH STEEL produces and exports JIS G 4401 SK105 plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for JIS G 4401 SK105

The items below follow JIS G 4401:2009. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard JIS G 4401:2009, Carbon tool steels
Official symbol SK105 (1983 reference symbol SK3)
Product form on this page Steel plate (鋼板). JIS G 4401:2009 also covers other product forms, including steel strip
How designations are listed Official symbols (種類の記号) in JIS G 4401:2009 Table 1
Steelmaking Killed steel. Unless otherwise specified, hot rolled or hot forged at a forging reduction ratio of 4S or more
Usual plate delivery As-hot-rolled unless otherwise specified (JIS G 4401:2009 clause 4)
Annealed plate Usual after cold rolling when that form is agreed (JIS G 4401:2009 clause 4)
Chemical analysis Heat analysis (溶鋼分析) to JIS G 4401:2009 Table 1. That edition does not set a separate product-analysis table
Plate hardness JIS G 4401:2009 Table 3, including columns for cold-rolled plate and strip when that form is agreed
Other-form hardness JIS G 4401:2009 Table 2 applies to annealed products other than plates and strips (Brinell)
Appearance of plate and strip Hot-rolled plate and strip: JIS G 3193 clause 7. Cold-rolled plate and strip: JIS G 3141 clause 12
Dimensions of plate and strip Hot-rolled plate and strip: JIS G 3193 (thickness tolerances in clause 5 apply below 160 mm; 160 mm and above by agreement). Plate flatness: JIS G 4401:2009 Table 6 for thickness below 160 mm; 160 mm and above by agreement. Cold-rolled plate and strip sizes: JIS G 3141; thickness tolerance A of JIS G 3141 Table 16
Decarburization of plate By agreement. JIS G 4401:2009 Table 7 depths apply to hot-rolled round bar only
Marking JIS G 4401:2009 clause 11: mark the symbol, heat or inspection number, manufacturer name or abbreviation, quantity or mass, and dimensions. Cold-rolled plate or strip adds a −C suffix after the symbol unless that suffix is omitted by agreement
Enquiry information Name the JIS G 4401 symbol, the edition required, plate as the product form, delivery condition, dimensions and any extra tests or document type
Inspection document When a report is requested and no document type is named, JIS G 4401:2009 refers to JIS G 0415 inspection document 2.3 or inspection certificate 3.1.B
Units Composition in percent by mass; hardness on the scales named in the tables
Our supply We produce and export SK105 plate to the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of JIS G 4401 SK105

JIS G 4401:2009 Table 1 is heat analysis. Elements not listed in that table shall not be added intentionally except as needed to finish the heat, unless agreed. Note a) of that table states that copper shall not exceed 0.25 %, chromium shall not exceed 0.30 % and nickel shall not exceed 0.25 %, as impurities.

Element SK105 heat analysis, JIS G 4401:2009 Table 1 (wt. %)
Carbon (C) 1.00–1.10
Silicon (Si) 0.10–0.35
Manganese (Mn) 0.10–0.50
Phosphorus (P) 0.030 max
Sulfur (S) 0.030 max
Copper (Cu), impurity max (note a) 0.25
Chromium (Cr), impurity max (note a) 0.30
Nickel (Ni), impurity max (note a) 0.25

Silicon, manganese, phosphorus and sulfur limits are the same for all eleven symbols in JIS G 4401:2009 Table 1. Carbon is the value that changes from symbol to symbol. The note a) impurity limits for copper, chromium and nickel also apply to every symbol.

Hardness and mechanical requirements for JIS G 4401 SK105

JIS G 4401:2009 specifies hardness, not a tensile-strength package. Table 3 is the hardness table for steel plates and strips. Table 2 (informative annealing temperature and Brinell hardness) applies to annealed products other than plates and strips.

Plate and strip hardness (JIS G 4401:2009 Table 3) SK105
As-hot-rolled hardness, HRC —
Annealed hardness, HRB —
Annealed hardness, HRC 31 max
Cold-rolled annealed hardness, HV 220 max
As-cold-rolled hardness, HV (informative) 220–310 (informative)

JIS G 4401:2009 Table 3 does not specify an as-hot-rolled HRC value for SK105. It does specify annealed HRC (31 max). If annealed plate hardness is required, write the annealed condition on the order.

For products other than plates and strips, if Brinell measurement is difficult, JIS G 4401:2009 allows Rockwell B or Vickers instead; those hardness values are then by agreement.

Other-form annealed hardness (JIS G 4401:2009 Table 2) SK105
Informative annealing temperature, °C 750–780, slow cool
Hardness after annealing, HBW 212 max

If cold-rolled plate or strip is agreed, JIS G 4401:2009 Table 3 specifies annealed hardness 220 max HV for SK105, and lists as-cold-rolled hardness 220–310 (informative) HV as an informative value. Quenched-and-tempered hardness is not a specified requirement in JIS G 4401:2009; a quench-and-temper hardness test may be agreed as an additional test.

Delivery conditions for JIS G 4401 SK105

JIS G 4401:2009 clause 4 sets the usual supply states:

  • Steel is made as killed steel and, unless otherwise specified, by hot rolling or hot forging at a forging reduction ratio of 4S or more.
  • Plates and strips are as-hot-rolled unless otherwise specified.
  • When plates and strips are cold-rolled by agreement, they are usually annealed.
  • Products other than plates and strips are usually annealed after hot rolling or hot forging.

An enquiry that only says “SK105 plate” should still name the delivery condition, because as-hot-rolled and annealed plate are not interchangeable supply states. The informative annealing temperature in JIS G 4401:2009 Table 2 for SK105 is 750–780 °C, slow cool.

For later tool hardening, JIS G 4401:2009 Annex JA (informative) lists a standard quench of 750–810 °C, water cool, and a temper of 150–200 °C, air cool, for SK105. Those temperatures are reference values, not as-delivered hardness.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

JIS G 4401:2009 does not specify a welding procedure. SK105 is a carbon tool steel (heat-analysis carbon 1.00–1.10 %). It is not selected as a welded construction plate in the way a structural or pressure-vessel grade would be.

Thermal cutting can harden the adjacent material. That heat-affected zone should be considered, and removed where later forming or finishing requires it. Any cutting or joining procedure should be qualified for the carbon content, thickness and delivery condition named on the order.

Form, appearance, dimensions and decarburization

JIS G 4401:2009 clause 7.2 sends hot-rolled plate and strip dimensions to JIS G 3193. Thickness tolerances in that reference apply below 160 mm; 160 mm and above are by agreement. Plate flatness is given in JIS G 4401:2009 Table 6 for thickness below 160 mm; 160 mm and above is by agreement.

Appearance of hot-rolled plate and strip follows JIS G 3193 clause 7. Appearance of cold-rolled plate and strip follows JIS G 3141 clause 12. Decarburization depth for plate is by agreement; JIS G 4401:2009 Table 7 depths apply to hot-rolled round bar only.

Numeric thickness, width, length and flatness limits should be stated on the purchase order and confirmed on the mill documents for the ordered edition.

Applications and specification limits

We produce and export SK105 plate for tools and dies that specify this JIS G 4401 symbol. Informative examples in JIS G 4401:2009 Table 1 include hacksaws, chisels, gauges, springs, press dies, jigs and cutting tools.

SK105 is a water-hardening carbon tool steel. Wear resistance, through-hardness after a later hardening cycle and toughness depend on the ordered condition, thickness and any agreed extra tests.

JIS G 4401 is a carbon tool-steel standard. It is not an alloy tool-steel specification such as JIS G 4404 or ASTM A681, not a high-speed specification such as JIS G 4403, and not an alloy structural plate specification such as ASTM A829. SK105 is not an automatic substitute for those products.

Compare JIS G 4401 SK105 with other steel plates

SK105 is a carbon tool steel plate. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
JIS G 4401 SK105 (this plate) Water-hardening carbon tool steel plate, heat-analysis carbon 1.00–1.10 % As-hot-rolled unless otherwise specified; annealing or cold rolling by agreement JIS G 4401:2009 Table 3: as-hot-rolled HRC —; annealed HRB —; annealed HRC 31 max. No tensile package is specified. Typical tools include hacksaws, chisels, gauges, springs, press dies, jigs and cutting tools A different official symbol or a structural alloy plate is not an automatic substitute
JIS G 4401 SK140 tool steel plate Water-hardening carbon tool steel plate, heat-analysis carbon 1.30–1.50 % As-hot-rolled unless otherwise specified; annealing or cold rolling by agreement JIS G 4401:2009 Table 3: as-hot-rolled HRC —; annealed HRB —; annealed HRC 34 max Typical tools include blade files and paper files A different official symbol from SK105, not an automatic substitute
JIS G 4401 SK120 tool steel plate Water-hardening carbon tool steel plate, heat-analysis carbon 1.15–1.25 % As-hot-rolled unless otherwise specified; annealing or cold rolling by agreement JIS G 4401:2009 Table 3: as-hot-rolled HRC —; annealed HRB —; annealed HRC 31 max Typical tools include drills, small punches, razors, metalworking files, cutting tools, hacksaws and springs A different official symbol from SK105, not an automatic substitute
ASTM A829 Grade 4140 Chromium-molybdenum alloy structural plate, usually ordered by heat chemistry AR, annealed, normalized, NT or QT as ordered No automatic as-delivered strength package; tensile or hardness only if specified and compatible Machinery and general engineering parts, often heat treated after cutting Not a carbon tool steel. Different chemistry, heat treatment and purpose from JIS G 4401 plate

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. Confirm chemistry, product form, delivery condition and hardness before any substitution.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
Japan JIS G 4401:2009 SK105 This plate. Water-hardening carbon tool steel with heat-analysis carbon 1.00–1.10 %. Hardness, not a tensile package, is specified. This product
Japan JIS G 4401:2009 Table 1 (1983 reference) SK3 Listed as the 1983 reference symbol opposite this designation in Table 1. Use the current symbol on new orders.
International ISO 4957:1999 C105U JIS G 4401:2009 Annex JB lists C105U opposite SK105 as a corresponding symbol. Annex JB notes that similar ISO chemistries differ slightly, so this is a near name. Near name only, not an automatic substitute.
United States — No direct counterpart specified ASTM carbon tool steels use a different designation system. Confirm chemistry, product form and hardness before any substitution.
China — No direct counterpart specified Chinese carbon tool steels use a different designation system. Confirm chemistry, product form and hardness before any substitution.

Why choose SHH STEEL for JIS G 4401 SK105

  • We produce and export JIS G 4401 SK105 carbon tool steel plate
  • We review the enquiry for edition, symbol, product form, delivery condition, dimensions and any extra tests
  • We keep plate hardness (JIS G 4401:2009 Table 3) distinct from the other-form hardness in JIS G 4401:2009 Table 2
  • We match documentation to what the purchase order requires

How to enquire for JIS G 4401 SK105 plate

Item What to specify
Standard and symbol JIS G 4401 SK105 and the edition required
Product form Plate
Delivery condition As-hot-rolled (the usual JIS G 4401:2009 supply state for plate and strip) or annealed; say if cold-rolled plate or strip is required
Dimensions Required thickness, width and length; we confirm production and export feasibility against the enquiry
Chemistry Heat analysis to JIS G 4401:2009 Table 1, or to another edition if specified
Hardness Plate hardness to JIS G 4401:2009 Table 3. Table 2 Brinell limits apply to products other than plate and strip
Decarburization Agree a depth for plate if the project needs one; JIS G 4401:2009 Table 7 applies to hot-rolled round bar
Other tests Ultrasonic examination, quench-and-temper hardness or other extra tests only when written on the order
Documentation State the inspection document type required by the project
Processing Cutting or other processing only when requested; thermal-cutting practice depends on carbon content, condition and thickness

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Does JIS G 4401 cover plate, or only bars?
Yes. JIS G 4401:2009 has separate hardness rules for steel plates and strips (clause 6.2 and Table 3) and separate appearance and dimension rules (clause 7.2, including Table 6 for plate flatness). It cites JIS G 3193 for hot-rolled plate and strip.
Which edition do the tables on this page follow?
They follow JIS G 4401:2009. Specify the edition required on the purchase order.
Is SK105 the same as SK3?
JIS G 4401:2009 Table 1 lists SK3 as the 1983 reference symbol. The current designation is SK105.
Is SK105 the same as ISO 4957 C105U?
No automatic substitute should be assumed. JIS G 4401:2009 Annex JB lists C105U as a corresponding international symbol and notes that similar ISO chemistries differ slightly.
What should a quotation enquiry include?
JIS G 4401 SK105, the edition required, plate as the product form, delivery condition, thickness by width by length, quantity, any agreed plate-decarburization or extra tests, and the inspection document required by the project.

Request a quotation

Contact SHH STEEL for a quotation for JIS G 4401 SK105 carbon tool steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the delivery condition: as-hot-rolled or annealed, and say if cold-rolled plate or strip is required. If your project requires a stated plate hardness, a decarburization depth, ultrasonic examination or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry and supply condition.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X