JIS G4053 SCM435 Steel Plate | SCM435 Cr-Mo Alloy Steel Plate | JIS G4053 Steel - SHH STEEL

JIS G4053 SCM435 Steel Plate | SCM435 Cr-Mo Alloy Steel Plate

SCM435 steel plate is a chromium-molybdenum alloy steel for machine structural use under JIS G4053:2023, whose official English title is Low-alloyed steels for machine structural use. The standard applies to products of uniform cross-section manufactured by hot rolling, hot forging and hot extruding, generally supplied for further forging, cutting and heat treatment; it does not apply to steel tubes. The usual product forms are bars and wire rod; hot-rolled plates and strips are covered by the standard (clauses 7.2 and 8.2) and plate is supplied by agreement. This page is written to JIS G4053:2023; confirm that this is the edition on the order, and confirm every chemical figure against the official published tables of that edition.
Grade
SCM435
Standard (writing edition)
JIS G4053:2023
Official English title
Low-alloyed steels for machine structural use
Table 2 carbon (ladle analysis, secondary-agreed)
0.33–0.38 %; confirm official 2023 tables
Table 2 manganese (ladle analysis, secondary-agreed)
0.60–0.90 %; confirm official 2023 tables
Table 2 chromium (ladle analysis, secondary-agreed)
0.90–1.20 %; confirm official 2023 tables
Table 2 molybdenum (ladle analysis, secondary-agreed)
0.15–0.30 %; confirm official 2023 tables
Typical use note
Machine structural use; not marked mainly for case hardening
Product forms
Usually bars and wire rod; plate by agreement (clauses 7.2, 8.2)
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of JIS G4053 SCM435 Steel Plate

SCM435 steel plate is a chromium-molybdenum alloy steel for machine structural use under JIS G4053:2023, whose official English title is Low-alloyed steels for machine structural use. The standard applies to products of uniform cross-section manufactured by hot rolling, hot forging and hot extruding, generally supplied for further forging, cutting and heat treatment; it does not apply to steel tubes. The usual product forms are bars and wire rod; hot-rolled plates and strips are covered by the standard (clauses 7.2 and 8.2) and plate is supplied by agreement. This page is written to JIS G4053:2023; confirm that this is the edition on the order, and confirm every chemical figure against the official published tables of that edition.

JIS G4053:2023 is not itself a tensile-strength standard. Mechanical properties are not tabulated as a basic grade requirement; if the purchaser specifies heat treatment, mechanical values may be agreed. This page does not invent tensile, yield or hardness figures. The ladle-analysis figures in this section are those on which agreeing secondary references coincide. The official published tables of JIS G4053:2023 were not inspected for this page and govern acceptance for orders to that edition. Buyers should confirm every figure against the official text of the edition stated on the order. This page does not present a prior edition as the 2023 normative table.

JIS G4053 SCM435 Steel Plate Material Specification

This page is written to JIS G4053:2023 (Edition 10). As of 12 November 2026, JIS G4053:2026 has been published (20 May 2026) and is recorded as replacing the 2023 edition. This page does not tabulate the published 2026 tables. Buyers should confirm which edition is stated on the order. The ladle-analysis figures in this section are those on which agreeing secondary references coincide. The official published tables of JIS G4053:2023 were not inspected for this page and govern acceptance for orders to that edition. Buyers should confirm every figure against the official text of the edition stated on the order. This page does not present a prior edition as the 2023 normative table.

JIS G4053 SCM435 Steel Plate is described by JIS G4053:2023. The official English title is “Low-alloyed steels for machine structural use.” The official 2023 Scope (inspected in the official English text of that edition) covers low-alloyed steels for machine structural use manufactured by hot rolling, hot forging and hot extruding, of uniform cross-section, generally supplied for further forging, cutting and heat treatment, and not applicable to steel tubes (steel tubes are covered by JIS G 3441). The 2023 edition is based on ISO 683-1:2016, ISO 683-2:2016, ISO 683-3:2022 and ISO 683-5:2017, MOD, with Annexes JA to JC unique to JIS.

Secondary references that agree (the 2023 and 2026 revision drafts) state that the steel is manufactured from killed steel; that products are supplied as-hot-rolled or as-hot-forged, unless the purchaser specifies heat treatment; that plates may alternatively be manufactured to Annex JC; and that plates and strips which cannot be hot-rolled because of thickness may be cold-rolled by agreement (usually annealed afterwards, with quality to Annex JB). Confirm those manufacturing rules against the official 2023 text.

JIS G4053 SCM435 Steel Plate Chemical Composition

Clause 6 of the agreeing 2023 revision draft requires the ladle (melt) analysis to comply with Table 2. The ladle-analysis figures in this section are those on which agreeing secondary references coincide. The official published tables of JIS G4053:2023 were not inspected for this page and govern acceptance for orders to that edition. Buyers should confirm every figure against the official text of the edition stated on the order. This page does not present a prior edition as the 2023 normative table.

Grade C Si Mn P max S max Ni max Cr Mo Cu max
SCM435 0.33–0.38 0.15–0.35 0.60–0.90 0.030 0.030 0.25 0.90–1.20 0.15–0.30 0.30

Values are mass fraction, %. Phosphorus, sulphur, nickel and copper are maxima. Silicon, manganese, chromium and molybdenum are specified ranges. Any alloy element not listed in the table shall not be intentionally added except for the purpose of finishing the molten steel. Product analysis, when agreed, uses the permitted deviations of JIS G 0321 Table 4 (alloy steel); this page does not tabulate those deviation values. Confirm every limit, including the molybdenum range and the product-analysis deviations, against the official 2023 text.

In the same agreeing references, SCM435 is not marked as a mainly case-hardening grade (that note applies to SCM415 and SCM420). Confirm the official 2023 wording.

JIS G4053 SCM435 Steel Plate Mechanical Properties

JIS G4053:2023, as described in the official 2023 Scope and in agreeing secondary references, is a chemical-composition and product-form standard for low-alloyed machine-structural steels. It does not tabulate a basic yield strength, tensile strength, elongation or impact-energy table for SCM435. This page does not invent those figures and does not borrow them from a related ASTM, ISO or GB/T grade.

The agreeing 2023 revision draft states that, when the purchaser specifies heat treatment, mechanical-property values may be agreed between the parties (note to the manufacturing clause). Any such values are an agreed requirement, not a default of the grade. Confirm the official 2023 wording and state any agreed mechanical properties on the order.

JIS G4053 SCM435 Steel Plate Delivery Conditions

Agreeing secondary references for the 2023 revision state that products are supplied as-hot-rolled or as-hot-forged, unless the purchaser specifies heat treatment. Do not assume a quenched-and-tempered or normalized delivery as a default. Confirm the official 2023 delivery wording.

The usual product forms under this standard are bars and wire rod. Hot-rolled plates and strips are specified in clauses 7.2 and 8.2; plate is supplied by agreement. Annex JC (normative), in the agreeing 2023 draft, requires plates to be manufactured by hot rolling at a forging-reduction ratio of 4S or more, unless a lower ratio is agreed. Ultrasonic testing may be agreed. Confirm Annex JC against the official 2023 text. Cold-rolled plate or strip, where agreed because thickness prevents hot rolling, is subject to Annex JB.

Order information in the agreeing 2023 draft (clause 12) requires the purchaser to state at least: the product form (bar, wire rod, plate, strip, flat, section or other, and the section type if applicable); the steel name (clause 4); the dimensions; and, for hot-rolled bars, the intended use (general forging, direct cutting, cold drawing, or other). Confirm the official 2023 list. Inspection documents, when required, follow JIS G 0404; if not otherwise specified at order, the default is an inspection certificate 3.1 under JIS G 0415.

JIS G4053 SCM435 Steel Plate Weldability

JIS G4053:2023 does not specify a welding procedure, a carbon equivalent or preheat for SCM435. A listed chemical composition is not a welding procedure. Any welding is a fabricator responsibility and shall be qualified to the project specification and to the official edition on the order. This page does not tabulate preheat or heat-input controls, and does not claim that the grade is, or is not, weldable as a general rule.

JIS G4053 SCM435 Steel Plate Tolerances

According to the agreeing 2023 revision draft, dimensions and tolerances of hot-rolled plates and strips follow JIS G 3193 (standard dimensions, shape and dimensional tolerances, and mass), and appearance follows JIS G 3193, with the application of weld repair and the maximum depth of remaining defects by agreement (clause 8.2). If cold rolling is agreed, Annex JB applies instead. Hot-rolled flats follow JIS G 3194. This page does not tabulate the numerical schedules of those dimensional standards. Confirm the official 2023 references and the ordered dimensional standard. A 2026 revision point on thickness tolerances at 160 mm and above is not presented here as a 2023 requirement.

JIS G4053 SCM435 Steel Plate Applications and service limits

SCM435 is a chromium-molybdenum alloy steel for machine structural use, generally supplied for further forging, cutting and heat treatment. It is not marked in the agreeing grade-symbol table as a mainly case-hardening grade. Selection of the grade, the thickness, the delivery condition and any agreed heat treatment or mechanical properties is a design decision for the project engineer. JIS G4053 does not by itself assign a minimum design temperature, a pressure-equipment duty, a fire rating or a fatigue class. Confirm fitness for the intended service against the official edition on the order, the project specification and the inspection document.

Inspection in the agreeing 2023 draft requires conformity of chemical composition (clause 6), shape, dimensions and mass (clause 7) and appearance (clause 8). General inspection matters follow JIS G 0404. Confirm those clauses against the official 2023 text.

Compare SCM435 with other JIS G4053 grades

SCM435 under JIS G4053:2023 is not a substitute for another G4053 grade, and a similar carbon range in another standard is not automatic equivalence. Confirm official 2023 tables before comparing compositions.

  • SCM430 — lower carbon (0.28–0.33 %) and the same molybdenum range (0.15–0.30 %); also not marked as mainly for case hardening. That product page is named, not linked. The relationship is not interchangeability.
  • SCM440 — higher carbon (0.38–0.43 %) and the same molybdenum range (0.15–0.30 %); also not marked as mainly for case hardening. That product page is named, not linked. The relationship is not interchangeability.
  • GB/T 11251 GB/T 11251 35CrMo is a commonly compared chromium-molybdenum alloy steel plate. Official correspondence tables were not inspected. A similar name is not interchangeability. Engineer approval is required before any substitution. Confirm both official texts.
  • ASTM A829/A829M ASTM A829 4135 is a commonly compared chromium-molybdenum alloy steel plate. Official correspondence tables were not inspected. A similar name is not interchangeability. Engineer approval is required before any substitution. Confirm both official texts.

JIS G4053 SCM435 Steel Plate Equivalent Material Grade

The heading identifies a comparison topic, not a declaration of interchangeable material. No formal equivalence has been verified. Official correspondence tables were not inspected. Compositions quoted on this page shall be confirmed against official JIS G4053:2023 tables before any comparison is used on an order.

Standard Country-Region Equivalent Grade Note
JIS G4053:2023 Japan SCM435 Chromium-molybdenum alloy steel for machine structural use on this page. Usual forms are bars and wire rod; plate by agreement. Confirm composition against the official 2023 tables. Not interchangeable with another G4053 grade.
GB/T 11251 China 35CrMo Commonly compared chromium-molybdenum alloy steel plate. Official correspondence tables were not inspected. Not an automatic equivalent. Engineer approval is required before any substitution. Confirm both official texts.
ASTM A829/A829M United States 4135 Commonly compared chromium-molybdenum alloy steel plate. Official correspondence tables were not inspected. Not an automatic equivalent. Engineer approval is required before any substitution. Confirm both official texts.

None of those relationships is interchangeability. Confirm every requirement against the official text of each standard named on the order, and obtain engineer approval before any substitution.

Why choose Us

SHH STEEL produces and exports alloy steel for machine structural use to JIS G4053, including supply of JIS G4053 SCM435 Steel Plate. We review the ordered edition, the steel name, the product form, the dimensions and any agreed heat treatment or mechanical properties before production, and we state the actual ladle analysis on the inspection document. We do not treat a related GB/T 11251 name as a JIS G4053 grade by default, and we confirm composition against the official edition on the order.

Orders are accepted against JIS G4053:2023 unless the order states a different edition, including JIS G4053:2026. See the JIS G4053 hub for the product family.

Our Service

Supply covers production to the ordered JIS G4053 requirements, mill documentation, and export packing and shipment. Inspection documents record the actual ladle analysis and any agreed mechanical results. Agreed options, including heat treatment and product analysis, are supplied when they are stated on the order, not by default. Usual product forms are bars and wire rod; plate is supplied by agreement.

To enquire, state the edition (JIS G4053:2023 or, if required, JIS G4053:2026), the steel name (SCM435), the product form and dimensions, the quantity, and any required heat treatment or agreed mechanical properties. SHH STEEL will confirm manufacturability against the official tables of the edition on the order. This page is a product description written to JIS G4053:2023; the official standard of the edition on the order, and the inspection document, govern acceptance.

FAQ

What is SCM435 steel plate?

JIS G4053 SCM435 Steel Plate is a chromium-molybdenum alloy steel for machine structural use under JIS G4053:2023. The usual product forms are bars and wire rod; plate is supplied by agreement, against the ladle-analysis limits of the official edition on the order. Confirm those limits against the official published tables of JIS G4053:2023. The grade is not specified by a tabulated tensile strength in that standard.

Is JIS G4053:2023 still current for SCM435?

This page is written to JIS G4053:2023. As of 12 November 2026, JIS G4053:2026 has been published (20 May 2026) and is recorded as replacing the 2023 edition. Confirm which edition applies to the order. This page does not tabulate the published 2026 tables. The official published tables of JIS G4053:2023 were not inspected for the grade chemistry on this page and govern acceptance for orders to 2023; confirm every figure against the official text. State the edition, the steel name, the product form and the dimensions on the order.

How does SCM435 differ from SCM430 and SCM440?

Agreeing secondary references give SCM435 a Table 2 carbon range of 0.33–0.38 % and a molybdenum range of 0.15–0.30 %; it is not marked mainly for case hardening. SCM430 has lower carbon (0.28–0.33 %) and the same molybdenum, chromium and manganese ranges, and is also not so marked. SCM440 has higher carbon (0.38–0.43 %) and the same molybdenum range, and is also not so marked. All three share silicon 0.15–0.35 %, manganese 0.60–0.90 % and chromium 0.90–1.20 % in those references, with the same residual maxima. The three grades are not interchangeable. Confirm every figure against official JIS G4053:2023 tables. Sibling product pages are named, not linked.

What information must be supplied on a JIS G4053 SCM435 order?

State the edition (JIS G4053:2023, or JIS G4053:2026 if that is required), the steel name (SCM435), the product form (bar, wire rod, plate, strip, flat, section or other), the dimensions and the quantity. For hot-rolled bars, state the intended use (general forging, direct cutting, cold drawing, or other). State any required heat treatment and any agreed mechanical properties, and any product analysis. Confirm the official order-information list of the edition on the order.

How should SCM435 steel plate be ordered?

State JIS G4053:2023, or JIS G4053:2026 if that is the edition required, and the steel name (SCM435). State whether the supply is bar, wire rod, or plate or strip by agreement, with the dimensions. State any agreed heat treatment, mechanical properties or product analysis. The official published tables of the edition on the order govern acceptance. The chemical figures on this page shall be confirmed against those official tables.

Enquire about JIS G4053 SCM435 Steel Plate

Enquire for JIS G4053 SCM435 Steel Plate to JIS G4053:2023, or state JIS G4053:2026 if that is the edition required. State the steel name (SCM435), the product form (including plate by agreement), the dimensions, the quantity and any agreed heat treatment or mechanical properties. SHH STEEL will confirm the inspection plan against the official tables of the edition on the order. The official standard and the inspection document govern acceptance.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response