JIS G 3101 SS490 Steel I-Beam
What is a JIS G 3101 SS490 Steel I-Beam?
A JIS G 3101 SS490 I-beam is a general-structure rolled I-section whose material conforms to JIS G 3101 and whose standard sizes follow JIS G 3192 Table 11. The grade is named for a 490 N/mm2 tensile minimum (the tabulated range is 490-610 N/mm2), not for a 490 N/mm2 yield. Yield is 285 N/mm2 up to 16 mm, based on flange thickness. This page is SS490 only, and only the I-section. It is not the live SS400 I-beam page, not the SS490 H-beam page, and not a JIS G 3106 SM490 product.
Material, Dimensions and Tolerances for JIS G 3101 SS490 I-Sections
JIS G 3101 is the material standard. JIS G 3192 is the dimensional standard; Table 11 is the I-section series used here, not Table 15 H-sections. Shape and mass tolerances follow JIS G 3192 as named on the order. The edition of each document on the contract governs acceptance. A mill may certify SS490 on a different series only when that combination is documented.
JIS G 3101 SS490 I-Beam Sizes: JIS G 3192 Table 11
The table lists the same 20 typographical I-sections already verified on the SS400 I-beam page, from I-100x75x5x8 to I-600x190x16x35. It is not a mill rolling list and not an H-beam table. Theoretical masses are those of Table 11. The designation, the grade and the dimensional standard all have to appear on the certificate.
Swipe horizontally to view all dimensions.
| Designation | H (mm) | B (mm) | t1 (mm) | t2 (mm) | r1 (mm) | r2 (mm) | A (cm²) | Mass (kg/m) |
|---|---|---|---|---|---|---|---|---|
| I-100×75×5×8 | 100 | 75 | 5 | 8 | 7 | 3.5 | 16.43 | 12.9 |
| I-125×75×5.5×9.5 | 125 | 75 | 5.5 | 9.5 | 9 | 4.5 | 20.45 | 16.1 |
| I-150×75×5.5×9.5 | 150 | 75 | 5.5 | 9.5 | 9 | 4.5 | 21.83 | 17.1 |
| I-150×125×8.5×14 | 150 | 125 | 8.5 | 14 | 13 | 6.5 | 46.15 | 36.2 |
| I-180×100×6×10 | 180 | 100 | 6 | 10 | 10 | 5 | 30.06 | 23.6 |
| I-200×100×7×10 | 200 | 100 | 7 | 10 | 10 | 5 | 33.06 | 26.0 |
| I-200×150×9×16 | 200 | 150 | 9 | 16 | 15 | 7.5 | 64.16 | 50.4 |
| I-250×125×7.5×12.5 | 250 | 125 | 7.5 | 12.5 | 12 | 6 | 48.79 | 38.3 |
| I-250×125×10×19 | 250 | 125 | 10 | 19 | 21 | 10.5 | 70.73 | 55.5 |
| I-300×150×8×13 | 300 | 150 | 8 | 13 | 12 | 6 | 61.58 | 48.3 |
| I-300×150×10×18.5 | 300 | 150 | 10 | 18.5 | 19 | 9.5 | 83.47 | 65.5 |
| I-300×150×11.5×22 | 300 | 150 | 11.5 | 22 | 23 | 11.5 | 97.88 | 76.8 |
| I-350×150×9×15 | 350 | 150 | 9 | 15 | 13 | 6.5 | 74.58 | 58.5 |
| I-350×150×12×24 | 350 | 150 | 12 | 24 | 25 | 12.5 | 111.1 | 87.2 |
| I-400×150×10×18 | 400 | 150 | 10 | 18 | 17 | 8.5 | 91.73 | 72.0 |
| I-400×150×12.5×25 | 400 | 150 | 12.5 | 25 | 27 | 13.5 | 122.1 | 95.8 |
| I-450×175×11×20 | 450 | 175 | 11 | 20 | 19 | 9.5 | 116.8 | 91.7 |
| I-450×175×13×26 | 450 | 175 | 13 | 26 | 27 | 13.5 | 146.1 | 115 |
| I-600×190×13×25 | 600 | 190 | 13 | 25 | 25 | 12.5 | 169.4 | 133 |
| I-600×190×16×35 | 600 | 190 | 16 | 35 | 38 | 19 | 224.5 | 176 |
JIS G 3101 SS490 Chemical Composition (Heat Analysis)
For SS490, only phosphorus and sulphur have specified maxima: 0.050 % each. Carbon and manganese are not specified. Do not invent a carbon cap, and do not copy the 0.30 % carbon and 1.60 % manganese limits of SS540 onto this grade.
Swipe horizontally to view all dimensions.
JIS G 3101 SS490 Mechanical Properties: Yield, Tensile, Elongation and Bend
Minimum yield is 285 N/mm2 up to 16 mm flange thickness, then 275, 255 and 245 N/mm2 in the usual bands, including thicknesses over 100 mm. Tensile strength is 490-610 N/mm2 in all those bands. Elongation and the 180-degree bend follow Table 3 as shown. JIS G 3101 does not specify a Charpy test for SS490; a toughness value must not be inferred from the grade name.
Swipe horizontally to view all dimensions.
Applications and Service Limits for JIS G 3101 SS490 Steel I-Beams
SS490 I-sections are used in general-structure frames and fabrication where this tensile class is specified in an I-beam. This page is not a design guide and does not give span tables. If the project needs a welded-structure grade (SM), a lower-temperature quality, or an H-section, nominate that product instead of stretching this certificate.
Near-Equivalents for JIS G 3101 SS490 Steel I-Beams: Not Automatic Substitutes
SS400 is a lower-tensile grade in the same standard, using the same Table 11 series. SS540 is a higher-tensile grade with a 40 mm mechanical cap and a specified carbon and manganese limit. SM490 is JIS G 3106, not G 3101. S355JR I-beams and Q355B I-beams use different shape systems as well as different material standards.
Sourcing JIS G 3101 SS490 Steel I-Beams from SHH STEEL
Send the Table 11 designation, the length, and the JIS G 3101 edition, and name SS490 explicitly. Do not use the SS400 I-beam term or the SS490 H-beam term for this page. SHH STEEL reviews the grade, the section and the certificate before quoting. The size table is a typographical reference, not a warehouse list.
JIS G 3101 SS490 I-Beam FAQs
-
Is this the same page as the SS490 H-beam?
- No. The grade is the same, but this page is the I-section to JIS G 3192 Table 11. H-sections use Table 15 and stay on the H-beam page.
-
Is the yield 490 N/mm2?
- No. 490 N/mm2 is the tensile minimum. Yield is 285 N/mm2 up to 16 mm flange thickness.
-
Does SS490 specify carbon?
- No. Only phosphorus and sulphur have maxima (0.050 %). Carbon and manganese are not specified for SS490.
-
Is a Charpy value included?
- No. JIS G 3101 does not specify a Charpy test for this grade. A toughness requirement has to be added on the order if it is needed.
Conclusion
JIS G 3101 SS490 I-beams use the 20 typographical Table 11 I-sections with a 490-610 N/mm2 tensile range and a 285 N/mm2 yield up to 16 mm. This is not the SS400 I-beam and not the SS490 H-beam. Confirm the designation, the grade and the certificate on the order.