ISO 4957 HS0-4-1 Tool Steel Plate | ISO 4957 Tool Steel - SHH STEEL

ISO 4957 HS0-4-1 Tool Steel Plate

ISO 4957 HS0-4-1 is a alloy high-speed tool steel for cutting-tool blanks, supported cutting inserts and tooling components. Its carbon range is 0.77–0.85 %, with the delivery condition and alloy balance defining the appropriate tooling route. Plate and flat blanks are selected by chemistry, surface quality, machining allowance and the actual section rather than by an unqualified foreign-grade nickname. Finished tooling still requires a qualified treatment and inspection basis. SHH STEEL produces and exports HS0-4-1 plate to the specified edition, dimensions and inspection requirements.
Equivalent Grades:
SKH51 contrast qualified; substitution requires review.
Heat Treatment
Annealed (+A).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is ISO 4957 HS0-4-1 plate?

ISO 4957 HS0-4-1 Tool Steel Plate is a alloy high-speed tool steel, associated with steel number 1.3325 in informative Annex C of ISO 4957:1999. The formal Table 8 row specifies chromium 3.90–4.40 % and vanadium 0.90–1.10 %, with its own carbon, alloy and reference-test requirements.

The numerical basis here is the finalized 1999 edition. Its broad wrought-product scope includes hot-rolled, forged, cold-drawn and cold-rolled products and permits powder metallurgy; plate and flat enquiries must identify the actual form and finish. This dated reference is not a statement that a later edition has identical requirements.

Tool geometry, carbide structure, grinding and production treatment require review; minimum specimen HRC is not guaranteed plate through-hardness, tool life or a service-temperature rating.

SHH STEEL produces and exports HS0-4-1 plate against the agreed specification and inspection basis. The standard hub is ISO 4957 within Tool and Die Steel Plates.

Material specification for HS0-4-1

Parameter Reference / scope
Standard / symbol ISO 4957:1999; HS0-4-1
Steel number 1.3325; informative Annex C, EN 10027-2:1992 designation
Family High-speed tool steel
Product form Broad wrought-product scope; state plate/flat, manufacture, dimensions and finish
Delivery condition Annealed (+A) unless otherwise specified
Condition hardness 262 HB maximum in annealed (+A) condition, Table 8
Hardening-test minimum 60 HRC on the prescribed test basis; not as-delivered plate HRC
Dimensions Agreement under clause 4.4; flat-bar references not automatic plate tolerances
Inspection Agreed document and test scope; ISO 10474 references as cited by the 1999 edition

Cast-analysis composition of HS0-4-1

Table 8 values below are cast-analysis requirements, mass percent. They are not product-analysis limits with an arbitrary extra allowance already included.

Element Cast-analysis requirement (wt. %)
Carbon (C) 0.77–0.85
Silicon (Si) 0.65 max
Manganese (Mn) 0.40 max
Phosphorus (P) 0.030 max
Sulfur (S) 0.030 max
Chromium (Cr) 3.90–4.40
Vanadium (V) 0.90–1.10
Molybdenum (Mo) 4.00–4.50

For product analysis use the applicable Table 9 deviations and sampling conditions. Elements not quoted must not be intentionally added without purchaser agreement except to finish the heat; precautions against additions from scrap/materials are required. A dash is not a zero-residual guarantee.

Table 9 product-analysis deviations are a separate acceptance basis, not a relaxation of the cast-analysis windows above.

Element Permissible product-analysis deviation (wt. %)
Carbon (C) ±0.03
Silicon (Si) +0.03
Manganese (Mn) +0.04
Phosphorus (P) +0.005
Sulfur (S) +0.005
Chromium (Cr) ±0.10
Vanadium (V) ±0.05
Molybdenum (Mo) ±0.10

Table 9 NOTE allows deviation either above or below the range, but not both for the same element from different sample products of the same cast. Maxima-only deviations are positive only. Values require ISO 14284 samples representing the average composition of the product cross-section.

Delivery hardness and hardening-test response for HS0-4-1

262 HB maximum in annealed (+A) condition, Table 8. The condition-specific Brinell maximum is different from the minimum HRC after the reference hardening test.

Property / regime Value / meaning
Delivery-condition Brinell basis 262 HB maximum in annealed (+A) condition, Table 8
Hardening-test minimum 60 HRC after the stipulated test treatment
Cold-worked stock Table 8 note d permits annealed+cold-drawn (+A+C) up to 50 HB above annealed, and annealed+cold-rolled (+A+CR) up to 70 HB above annealed; neither is an annealed-plate allowance
Final tool hardness Specified separately for the real section and production treatment

Table 1 note c adds the minimum-hardness hardening-test requirements. Supplementary verification is defined by normative Annex B.3, with Annex B.1 requiring supplementary/special items to be specified at enquiry and order. These numerical minima are not an informative tempering-curve estimate or a blanket finished-tool guarantee.

Delivery condition and test treatment for HS0-4-1

Specify Annealed (+A) unless otherwise specified. Clause 4.1.2.1 gives annealed delivery unless otherwise specified. A separate production heat treatment must be qualified for the actual tool.

Table 8 / Annex B.3 hardening-test item Reference
Hardening temperature 1120 °C (±10 °C)
Quench medium Oil or salt bath; oil only in dispute
Minimum reference tempering temperature 560 °C minimum (±10 °C table tolerance)
Minimum test hardness 60 HRC
Salt-bath total heating, Table B.1 3 min for hardening; minimum 2 tempering periods of 60 min each
Other heating methods Extend the heating time accordingly; no universal production holding time assigned

B.3 requires the Figure 1 test-piece location, conditions avoiding decarburization, and hardness measurement on the prepared cut surface to ISO 6508. Untreated samples may be annealed before the test at the manufacturer’s discretion. No preheat temperature is specified by these rows, so none is inferred. These are specimen-test conditions, not guaranteed production recipes for every plate section. Annex A hardness-tempering curves are informative guidance, not identical acceptance limits.

Table 8 note e permits oil or salt bath for the reference hardening test; in dispute only oil is used. Usual quenching media in practice are air, gas or salt bath. These alternatives do not turn a specimen test into a universal production recipe. The printed tempering temperature is a minimum reference with the stated table tolerance.

Welding, cutting and finishing HS0-4-1

HS0-4-1 tool steel requires a qualified repair-welding procedure matched to chemistry, supplied condition, restraint and final treatment; it is not a generic readily weldable fabrication plate. No unsourced welding temperature is prescribed.

Thermal cutting, EDM and grinding can change the surface layer and introduce damage. Review cleanup allowance, inspect critical edges and avoid representing an unaffected core analysis as proof of sound tool surfaces. Tool geometry, carbide structure, grinding and production treatment require review; minimum specimen HRC is not guaranteed plate through-hardness, tool life or a service-temperature rating.

Plate/flat dimensions and surface acceptance

Clause 4.4 requires shape, dimensions and tolerances agreed at enquiry and order, preferably using corresponding international or suitable national standards. ISO 1035-1/-3/-4 are cited for rolled round and flat bars; their bar tolerances must not simply be relabelled as plate tolerances. No invented plate capacity range, thickness deviation or flatness number is supplied here.

Clause 4.3 requires a workmanlike surface. Ground, polished or finished-machined products are to be free of surface imperfections and surface decarburization. Hot-rolled, forged, cold-drawn or rough-machined stock requires sufficient cleanup material; machining allowance is agreed under the 1999 provisions. Do not transfer round-product hardenability or surface limits to plate without the appropriate basis.

Applications and selection limits for HS0-4-1

Qualitative engineering applications for HS0-4-1 include cutting-tool blanks, supported cutting inserts and tooling components. The formal Table 8 row specifies chromium 3.90–4.40 % and vanadium 0.90–1.10 %, with its own carbon, alloy and reference-test requirements. The actual finished tool, duty and edge support must be reviewed rather than assumed from a grade nickname.

Tool geometry, carbide structure, grinding and production treatment require review; minimum specimen HRC is not guaranteed plate through-hardness, tool life or a service-temperature rating.

The standard’s condition hardness and hardening-test response do not provide a numerical impact property, corrosion rating or guaranteed tool life. High carbon or alloy content alone is not a substitute for a drawing and final acceptance requirements.

Compare HS0-4-1 with three published own plates

These own product pages are already live. The following comparisons are material-selection contrasts, not automatic substitution approvals.

Material Family / chemistry Condition Property basis Substitution limit
HS0-4-1 (this plate) alloy high-speed tool steel 262 HB maximum in annealed (+A) condition, Table 8 Minimum specimen-test 60 HRC, not as-delivered plate hardness Condition/form/test basis must match
JIS G4401 SK105 Tool Steel Plate Carbon tool steel; published C 1.00–1.10 % JIS G4401:2009 plate/strip condition basis; as-hot-rolled unless otherwise specified Not the ISO 4957:1999 Table 8 specimen-test acceptance Compare actual carbon, Si/Mn limits, condition and plate rules
JIS G4401 SK120 Tool Steel Plate Carbon tool steel; published C 1.15–1.25 % JIS G4401:2009 plate/strip condition basis; as-hot-rolled unless otherwise specified Not the ISO 4957:1999 Table 8 specimen-test acceptance Compare actual carbon, Si/Mn limits, condition and plate rules
ASTM A829 4140 Alloy Steel Plate Engineering Cr-Mo plate; separate chemistry-ordered specification Ordered condition on the own live page Chemistry-ordered engineering plate, not this tool-test acceptance Not a direct tool-grade substitute

Country comparisons and substitution limits for HS0-4-1

The country comparison uses actual cited editions, not an unrestricted trade-name list. The steel number is the informative Annex C designation association, not proof that foreign delivery and test requirements are identical.

System Grade / number Actual chemistry / form difference Condition / substitution limit
ISO / international HS0-4-1 Cast-analysis Table 8; this grade and edition Delivery condition, specimen response and plate/flat requirements must be specified
Europe / designation number 1.3325 Informative Annex C associates the EN 10027-2:1992 number; it is not an independently verified later DIN specification No automatic national-edition or product-condition certification inferred
Japan JIS G4403:2015 SKH51 contrast JIS C 0.80–0.88, Mo 4.70–5.20, V 1.70–2.10 and W 5.90–6.70 versus ISO C 0.77–0.85, Mo 4.00–4.50, V 0.90–1.10 and no quoted W range. No direct JIS counterpart established; a high-speed family contrast only.

The ISO hardening-test HRC is a genuine specimen-response basis. It must not be confused with JIS G4404 practical-decarburization HV criteria, JIS plate delivery hardness or an informative tempering curve. Verify the complete foreign standard, form and ordered condition before substitution.

Why choose SHH STEEL for HS0-4-1

SHH STEEL produces and exports HS0-4-1 plate against the stated standard, supplied condition and agreed inspection plan. We keep cast analysis, delivery hardness and final tooling acceptance distinct.

  • Confirm the required edition and correct material designation.
  • Use plate/flat tolerances and cleanup allowance appropriate to the actual form.
  • Agree supplementary verification and required reports before acceptance.
  • Maintain heat identification and review any proposed foreign substitution.

Enquiry and inspection planning for HS0-4-1

Enquiry item What to specify
Grade / edition HS0-4-1; ISO edition and any associated drawing requirement
Form / dimensions Plate or flat, thickness × width × length, quantity, finish and machining allowance
Condition Annealed (+A) unless otherwise specified
Hardness basis 262 HB maximum in annealed (+A) condition, Table 8
Verification State whether Annex B.3 hardening verification, product analysis or other supplementary tests are required
Final tooling Actual tool duty, final property acceptance and production-treatment responsibility
Reports / logistics Inspection-document type, heat traceability, packing, destination and target timing

Dimensions, manufacturing route and any additional NDT or quality requirement are reviewed for feasibility. This page is not an unconditional stock, capacity or finished-tool performance commitment.

FAQ

What distinguishes HS0-4-1?
The formal Table 8 row specifies chromium 3.90–4.40 % and vanadium 0.90–1.10 %, with its own carbon, alloy and reference-test requirements. Tool geometry, carbide structure, grinding and production treatment require review; minimum specimen HRC is not guaranteed plate through-hardness, tool life or a service-temperature rating.
Does the HRC value describe supplied plate?
No. The reference hardening test gives 60 HRC minimum on its stipulated specimen basis. The delivery-condition entry is 262 HB maximum in annealed (+A) condition, Table 8. Final tool properties require a separate qualified basis.
Are these temperatures a production heat-treatment guarantee?
No. The table/B.3 regime is a specimen test. Table 1 note c provides the minimum-response requirement, while Annex B.1 makes supplementary verification an enquiry/order item. Annex A curves are informative; actual tool treatment depends on section and application.
Can round hardenability or bar tolerances be used directly for plate?
No. Follow the actual product-form agreement under clause 4.4 and Figure 1 sample rules. Any Table 2 round-diameter hardenability statements are not plate-thickness guarantees.
Is the foreign grade or steel number an automatic equivalent?
No. Use the explicit country-table differences, complete source edition, actual form, delivery condition and test acceptance. Historical JIS names and informative steel-number associations do not establish unconditional substitution.

Request a quotation

Request a quotation for ISO 4957 HS0-4-1 tool steel plate or flat stock. Send the required edition, quantity, dimensions, finish, machining allowance and drawing. State the supplied condition explicitly: Annealed (+A) unless otherwise specified. Identify the intended tooling duty and whether dimensions describe raw blanks or finished pieces.

Include the delivery-hardness acceptance, required inspection document and heat-traceability needs. Specify any supplementary product analysis, Annex B.3 hardening-test verification, surface/decarburization evaluation or additional NDT, with the agreed method and acceptance criteria. Do not treat a specimen-response HRC or round-diameter hardenability note as an arbitrary-section plate guarantee.

Provide the final tool properties and production-treatment responsibility separately. For a proposed foreign grade, attach its governing specification and drawing so chemistry, form and condition differences can be reviewed. Include cutting details, edge preparation, inspection stages, destination, packing and target timing; requested processes and dimensions are reviewed for feasibility before confirmation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X