ISO 4957 21MnCr5 Tool Steel Plate
What is ISO 4957 21MnCr5 plate?
ISO 4957 21MnCr5 Tool Steel Plate is a low-carbon manganese-chromium carburizing tool steel, associated with steel number 1.2162 in informative Annex C of ISO 4957:1999. Its low-carbon core route is distinct from high-carbon through-hardened tooling; Table 4 footnote e addresses a carburized surface.
The numerical basis here is the finalized 1999 edition. Its broad wrought-product scope includes hot-rolled, forged, cold-drawn and cold-rolled products and permits powder metallurgy; plate and flat enquiries must identify the actual form and finish. This dated reference is not a statement that a later edition has identical requirements.
The surface-hardness reference after carburizing is not supplied-stock hardness, core hardness or a guarantee of a specified case depth.
SHH STEEL produces and exports 21MnCr5 plate against the agreed specification and inspection basis. The standard hub is ISO 4957 within Tool and Die Steel Plates.
Material specification for 21MnCr5
| Parameter | Reference / scope |
|---|---|
| Standard / symbol | ISO 4957:1999; 21MnCr5 |
| Steel number | 1.2162; informative Annex C, EN 10027-2:1992 designation |
| Family | Alloy cold-work tool steel |
| Product form | Broad wrought-product scope; state plate/flat, manufacture, dimensions and finish |
| Delivery condition | Annealed (+A) unless otherwise specified |
| Condition hardness | 217 HB maximum in annealed (+A) condition, Table 4 |
| Carburized surface reference | Table 4 footnote e: 60 HRC surface after carburizing, quenching and tempering; not a printed bulk-test minimum |
| Dimensions | Agreement under clause 4.4; flat-bar references not automatic plate tolerances |
| Inspection | Agreed document and test scope; ISO 10474 references as cited by the 1999 edition |
Cast-analysis composition of 21MnCr5
Table 4 values below are cast-analysis requirements, mass percent. They are not product-analysis limits with an arbitrary extra allowance already included.
| Element | Cast-analysis requirement (wt. %) |
|---|---|
| Carbon (C) | 0.18–0.24 |
| Silicon (Si) | 0.15–0.35 |
| Manganese (Mn) | 1.10–1.40 |
| Phosphorus (P) | 0.030 max |
| Sulfur (S) | 0.030 max |
| Chromium (Cr) | 1.00–1.30 |
For product analysis use the applicable Table 5 deviations and sampling conditions. Elements not quoted must not be intentionally added without purchaser agreement except to finish the heat; precautions against additions from scrap/materials are required. A dash is not a zero-residual guarantee.
Table 5 product-analysis deviations are a separate acceptance basis, not a relaxation of the cast-analysis windows above.
| Element | Permissible product-analysis deviation (wt. %) |
|---|---|
| Carbon (C) | ±0.03 |
| Silicon (Si) | ±0.03 |
| Manganese (Mn) | ±0.08 |
| Chromium (Cr) | ±0.05 |
| Phosphorus (P) | +0.005 |
| Sulfur (S) | +0.005 |
Table 5 note a allows deviation either above or below the range, but not both for the same element from different sample products of the same cast. Maxima-only deviations are positive only. Values require ISO 14284 samples representing the average composition of the product cross-section.
Delivery hardness and hardening-test response for 21MnCr5
Table 4 lists annealed (+A) hardness of 217 HB maximum. Footnote e says the material, when carburized, quenched and tempered, should achieve a surface hardness of 60 HRC. This is a processed surface reference, not annealed-stock HRC, core hardness or a numerical through-hardening minimum.
| Property / regime | Source basis |
|---|---|
| Annealed delivery | 217 HB maximum |
| Carburized surface | 60 HRC after carburizing, quenching and tempering; Table 4 footnote e |
| Ordinary hardening-test row | No hardening temperature, quench medium or tempering temperature is printed for 21MnCr5 |
| Case/core or through-hardness | Agree the applicable source, depth, specimen/section and acceptance; no value inferred |
Table 4 note c permits annealed plus cold-drawn (+A+C) hardness up to 20 HB above annealed (+A), not an annealed-plate allowance. Table 1 note c and supplementary verification under Annex B.3 selected under Annex B.1 do not supply a missing carburizing recipe. Annex A curves are informative and do not replace the qualified case-hardening reference.
Delivery condition and test treatment for 21MnCr5
21MnCr5 is annealed (+A) unless otherwise specified under clause 4.1.2.1. Keep supplied machining stock distinct from the carburized, quenched and tempered final component.
Table 4 refers the ordinary hardening/tempering test cells to footnote e rather than printing a numerical cycle or specified quench medium; note e provides the 60 HRC processed-surface reference. No carburizing temperature, case depth, holding time, preheat, quench medium or tempering recipe is inferred from a neighboring row.
Table B.1 gives general salt-bath specimen heating for the standard hardening test; it is not a complete carburizing treatment and cannot fill the blank 21MnCr5 row. Agree the final case/core requirements, treatment responsibility and verification against the applicable source and order. These are not guaranteed production recipes for arbitrary plate sections.
Welding, cutting and finishing 21MnCr5
21MnCr5 tool steel requires a qualified repair-welding procedure matched to chemistry, supplied condition, restraint and final treatment; it is not a generic readily weldable fabrication plate. No unsourced welding temperature is prescribed.
Thermal cutting, EDM and grinding can change the surface layer and introduce damage. Review cleanup allowance, inspect critical edges and avoid representing an unaffected core analysis as proof of sound tool surfaces. The surface-hardness reference after carburizing is not supplied-stock hardness, core hardness or a guarantee of a specified case depth.
Plate/flat dimensions and surface acceptance
Clause 4.4 requires shape, dimensions and tolerances agreed at enquiry and order, preferably using corresponding international or suitable national standards. ISO 1035-1/-3/-4 are cited for rolled round and flat bars; their bar tolerances must not simply be relabelled as plate tolerances. No invented plate capacity range, thickness deviation or flatness number is supplied here.
Clause 4.3 requires a workmanlike surface. Ground, polished or finished-machined products are to be free of surface imperfections and surface decarburization. Hot-rolled, forged, cold-drawn or rough-machined stock requires sufficient cleanup material; machining allowance is agreed under the 1999 provisions. Do not transfer round-product hardenability or surface limits to plate without the appropriate basis.
Applications and selection limits for 21MnCr5
Qualitative engineering applications for 21MnCr5 include case-hardened tool components and cold-tool blanks. Its low-carbon core route is distinct from high-carbon through-hardened tooling; Table 4 footnote e addresses a carburized surface. The actual finished tool, duty and edge support must be reviewed rather than assumed from a grade nickname.
The surface-hardness reference after carburizing is not supplied-stock hardness, core hardness or a guarantee of a specified case depth.
The standard’s condition hardness and hardening-test response do not provide a numerical impact property, corrosion rating or guaranteed tool life. High carbon or alloy content alone is not a substitute for a drawing and final acceptance requirements.
Compare 21MnCr5 with three published own plates
These own product pages are already live. The following comparisons are material-selection contrasts, not automatic substitution approvals.
| Material | Family / chemistry | Condition | Property basis | Substitution limit |
|---|---|---|---|---|
| 21MnCr5 (this plate) | low-carbon manganese-chromium carburizing tool steel | 217 HB maximum in annealed (+A) condition, Table 4 | 60 HRC carburized/quenched/tempered surface reference; not as-delivered or core hardness | Condition/form/test basis must match |
| JIS G4401 SK140 Tool Steel Plate | Carbon tool steel; published C 1.30–1.50 % | JIS G4401:2009 plate/strip condition basis; as-hot-rolled unless otherwise specified | Not the ISO 4957:1999 Table 2/4 specimen test | Compare actual carbon, Si/Mn limits, condition and plate rules |
| JIS G4401 SK120 Tool Steel Plate | Carbon tool steel; published C 1.15–1.25 % | JIS G4401:2009 plate/strip condition basis; as-hot-rolled unless otherwise specified | Not the ISO 4957:1999 Table 2/4 specimen test | Compare actual carbon, Si/Mn limits, condition and plate rules |
| ASTM A829 4140 Alloy Steel Plate | Engineering Cr-Mo plate; separate chemistry-ordered specification | Ordered condition on the own live page | Chemistry-ordered engineering plate, not this tool-test acceptance | Not a direct tool-grade substitute |
Country comparisons and substitution limits for 21MnCr5
The country comparison uses actual cited editions, not an unrestricted trade-name list. The steel number is the informative Annex C designation association, not proof that foreign delivery and test requirements are identical.
| System | Grade / number | Actual chemistry / form difference | Condition / substitution limit |
|---|---|---|---|
| ISO / international | 21MnCr5 | Cast-analysis Table 4; this grade and edition | Delivery condition, specimen response and plate/flat requirements must be specified |
| Europe / designation number | 1.2162 | Informative Annex C associates the EN 10027-2:1992 number; it is not an independently verified later DIN specification | No automatic national-edition or product-condition certification inferred |
| United States | ASTM A681-08 P2 | ASTM C 0.10 maximum versus ISO C 0.18–0.24; ASTM Cr 0.75–1.25 versus ISO 1.00–1.30. P2 requires Mo 0.15–0.40 and Ni 0.10–0.50, which are not quoted in this ISO row. | Low-carbon carburizing-mould contrast only. ASTM P-type response exemption does not replace the ISO footnote-e surface reference. |
For 21MnCr5 the ISO reference is the Table 4 footnote-e carburized-surface expectation, not a printed ordinary bulk hardening-test minimum. It must not be confused with JIS G4404 practical-decarburization HV criteria, JIS plate delivery hardness or an informative tempering curve. Verify the complete foreign standard, form and ordered condition before substitution.
Why choose SHH STEEL for 21MnCr5
SHH STEEL produces and exports 21MnCr5 plate against the stated standard, supplied condition and agreed inspection plan. We keep cast analysis, delivery hardness and final tooling acceptance distinct.
- Confirm the required edition and correct material designation.
- Use plate/flat tolerances and cleanup allowance appropriate to the actual form.
- Agree supplementary verification and required reports before acceptance.
- Maintain heat identification and review any proposed foreign substitution.
Enquiry and inspection planning for 21MnCr5
| Enquiry item | What to specify |
|---|---|
| Grade / edition | 21MnCr5; ISO edition and any associated drawing requirement |
| Form / dimensions | Plate or flat, thickness × width × length, quantity, finish and machining allowance |
| Condition | Annealed (+A) unless otherwise specified |
| Hardness basis | 217 HB maximum in annealed (+A) condition, Table 4 |
| Verification | State whether Annex B.3 hardening verification, product analysis or other supplementary tests are required |
| Final tooling | Actual tool duty, final property acceptance and production-treatment responsibility |
| Reports / logistics | Inspection-document type, heat traceability, packing, destination and target timing |
Dimensions, manufacturing route and any additional NDT or quality requirement are reviewed for feasibility. This page is not an unconditional stock, capacity or finished-tool performance commitment.
FAQ
-
What distinguishes 21MnCr5?
- Its low-carbon core route is distinct from high-carbon through-hardened tooling; Table 4 footnote e addresses a carburized surface. The surface-hardness reference after carburizing is not supplied-stock hardness, core hardness or a guarantee of a specified case depth.
-
Does the reference mean 60 HRC supplied plate?
- No. Annealed delivery is 217 HB maximum. Table 4 footnote e refers to a surface hardness of 60 HRC after carburizing, quenching and tempering; no supplied-stock HRC, core hardness or case depth is assigned.
-
What exact heat-treatment cycle is specified?
- No ordinary hardening temperature, quench medium or tempering temperature is printed for this row. Agree the applicable case-hardening source, final requirements and verification; general specimen heating in Table B.1 is not a complete carburizing recipe.
-
Can bar tolerances or surface hardness guarantee plate performance?
- No. Use actual plate/flat dimensional agreements under clause 4.4. The surface reference does not define plate through-hardness, case depth or core properties; these need the governing order and section basis.
-
Is P2 or another foreign carburizing grade equivalent?
- Not automatically. ASTM A681-08 P2 has C 0.10 maximum, Cr 0.75–1.25 and mandatory Mo/Ni ranges, unlike this ISO C 0.18–0.24 and Cr 1.00–1.30 row. Match full chemistry, form, supplied condition and final acceptance.
Request a quotation
Request a quotation for ISO 4957 21MnCr5 tool steel plate or flat stock. Send the required edition, quantity, dimensions, finish, machining allowance and drawing. State the supplied condition explicitly: Annealed (+A) unless otherwise specified. Identify the intended tooling duty and whether dimensions describe raw blanks or finished pieces.
Include the delivery-hardness acceptance, required inspection document and heat-traceability needs. Specify any supplementary product analysis, Annex B.3 hardening-test verification, surface/decarburization evaluation or additional NDT, with the agreed method and acceptance criteria. Do not treat a specimen-response HRC or round-diameter hardenability note as an arbitrary-section plate guarantee.
Provide the final tool properties and production-treatment responsibility separately. For a proposed foreign grade, attach its governing specification and drawing so chemistry, form and condition differences can be reviewed. Include cutting details, edge preparation, inspection stages, destination, packing and target timing; requested processes and dimensions are reviewed for feasibility before confirmation.
For 21MnCr5, specify the applicable carburizing source and required case/core acceptance, depth and measurement stage. The Table 4 surface reference is not a complete treatment cycle or a core-property guarantee.
Contact: admin@steelspecs.com