ISO 4957 C45U Tool Steel Plate | ISO 4957 Tool Steel - SHH STEEL

ISO 4957 C45U Tool Steel Plate

ISO 4957 C45U is a non-alloy medium-carbon cold-work tool steel for general-purpose tool blanks, fixtures and tooling supports. Its carbon range is 0.42–0.50 %, with the delivery condition and alloy balance defining the appropriate tooling route. Plate and flat blanks are selected by chemistry, surface quality, machining allowance and the actual section rather than by an unqualified foreign-grade nickname. Finished tooling still requires a qualified treatment and inspection basis. SHH STEEL produces and exports C45U plate to the specified edition, dimensions and inspection requirements.
Equivalent Grades:
Related grades; substitution requires review.
Heat Treatment
Non-heat-treated (+U).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is ISO 4957 C45U plate?

ISO 4957 C45U Tool Steel Plate is a non-alloy medium-carbon cold-work tool steel, associated with steel number 1.1730 in informative Annex C of ISO 4957:1999. The non-heat-treated delivery route distinguishes it from the higher-carbon water-hardening grades; do not assume an annealed default.

The numerical basis here is the finalized 1999 edition. Its broad wrought-product scope includes hot-rolled, forged, cold-drawn and cold-rolled products and permits powder metallurgy; plate and flat enquiries must identify the actual form and finish. This dated reference is not a statement that a later edition has identical requirements.

Its carbon window and untreated-use note do not make it a replacement for high-carbon cutting tools.

SHH STEEL produces and exports C45U plate against the agreed specification and inspection basis. The standard hub is ISO 4957 within Tool and Die Steel Plates.

Material specification for C45U

Parameter Reference / scope
Standard / symbol ISO 4957:1999; C45U
Steel number 1.1730; informative Annex C, EN 10027-2:1992 designation
Family Non-alloy cold-work tool steel
Product form Broad wrought-product scope; state plate/flat, manufacture, dimensions and finish
Delivery condition Non-heat-treated (+U); Table 2 footnote c
Condition hardness 207 HB maximum; Table 2 entry bears the untreated-use footnote c, not an annealed-default claim
Hardening-test minimum 54 HRC on the prescribed test basis; not as-delivered plate HRC
Dimensions Agreement under clause 4.4; flat-bar references not automatic plate tolerances
Inspection Agreed document and test scope; ISO 10474 references as cited by the 1999 edition

Cast-analysis composition of C45U

Table 2 values below are cast-analysis requirements, mass percent. They are not product-analysis limits with an arbitrary extra allowance already included.

Element Cast-analysis requirement (wt. %)
Carbon (C) 0.42–0.50
Silicon (Si) 0.15–0.40
Manganese (Mn) 0.60–0.80
Phosphorus (P) 0.030 max
Sulfur (S) 0.030 max

For product analysis use the applicable Table 3 deviations and sampling conditions. Elements not quoted must not be intentionally added without purchaser agreement except to finish the heat; precautions against additions from scrap/materials are required. A dash is not a zero-residual guarantee.

Delivery hardness and hardening-test response for C45U

207 HB maximum; Table 2 entry bears the untreated-use footnote c, not an annealed-default claim. The condition-specific Brinell maximum is different from the minimum HRC after the reference hardening test.

Property / regime Value / meaning
Delivery-condition Brinell basis 207 HB maximum; Table 2 entry bears the untreated-use footnote c, not an annealed-default claim
Hardening-test minimum 54 HRC after the stipulated test treatment
Cold-drawn stock The applicable table note permits annealed plus cold-drawn (+A+C) hardness up to 20 HB higher than annealed (+A); do not transfer this allowance to annealed plate or an untreated C45U basis
Final tool hardness Specified separately for the real section and production treatment

Table 1 note c adds the minimum-hardness hardening-test requirements. Supplementary verification is defined by normative Annex B.3, with Annex B.1 requiring supplementary/special items to be specified at enquiry and order. These numerical minima are not an informative tempering-curve estimate or a blanket finished-tool guarantee.

Delivery condition and test treatment for C45U

Specify Non-heat-treated (+U); Table 2 footnote c. Clause 4.1.2.1 excepts C45U from the ordinary annealed default; Table 2 footnote c states that this grade is used in the non-heat-treated condition.

Table 2 / Annex B.3 hardening-test item Reference
Hardening temperature 810 °C (±10 °C)
Quench medium Water
Tempering temperature 180 °C (±10 °C)
Minimum test hardness 54 HRC
Salt-bath total heating, Table B.1 25 ± 1 min for hardening; 60 min for tempering
Other heating methods Extend the heating time accordingly; no universal production holding time assigned

B.3 requires the Figure 1 test-piece location, conditions avoiding decarburization, and hardness measurement on the prepared cut surface to ISO 6508. Untreated samples may be annealed before the test at the manufacturer’s discretion. No preheat temperature is specified by these rows, so none is inferred. These are specimen-test conditions, not guaranteed production recipes for every plate section. Annex A hardness-tempering curves are informative guidance, not identical acceptance limits.

Welding, cutting and finishing C45U

C45U tool steel requires a qualified repair-welding procedure matched to chemistry, supplied condition, restraint and final treatment; it is not a generic readily weldable fabrication plate. No unsourced welding temperature is prescribed.

Thermal cutting, EDM and grinding can change the surface layer and introduce damage. Review cleanup allowance, inspect critical edges and avoid representing an unaffected core analysis as proof of sound tool surfaces. Its carbon window and untreated-use note do not make it a replacement for high-carbon cutting tools.

Plate/flat dimensions and surface acceptance

Clause 4.4 requires shape, dimensions and tolerances agreed at enquiry and order, preferably using corresponding international or suitable national standards. ISO 1035-1/-3/-4 are cited for rolled round and flat bars; their bar tolerances must not simply be relabelled as plate tolerances. No invented plate capacity range, thickness deviation or flatness number is supplied here.

Clause 4.3 requires a workmanlike surface. Ground, polished or finished-machined products are to be free of surface imperfections and surface decarburization. Hot-rolled, forged, cold-drawn or rough-machined stock requires sufficient cleanup material; machining allowance is agreed under the 1999 provisions. Do not transfer round-product hardenability or surface limits to plate without the appropriate basis.

Applications and selection limits for C45U

Qualitative engineering applications for C45U include general-purpose tool blanks, fixtures and tooling supports. The non-heat-treated delivery route distinguishes it from the higher-carbon water-hardening grades; do not assume an annealed default. The actual finished tool, duty and edge support must be reviewed rather than assumed from a grade nickname.

Its carbon window and untreated-use note do not make it a replacement for high-carbon cutting tools.

The standard’s condition hardness and hardening-test response do not provide a numerical impact property, corrosion rating or guaranteed tool life. High carbon or alloy content alone is not a substitute for a drawing and final acceptance requirements.

Compare C45U with three published own plates

These own product pages are already live. The following comparisons are material-selection contrasts, not automatic substitution approvals.

Material Family / chemistry Condition Property basis Substitution limit
C45U (this plate) non-alloy medium-carbon cold-work tool steel 207 HB maximum; Table 2 entry bears the untreated-use footnote c, not an annealed-default claim Minimum specimen-test 54 HRC, not as-delivered plate hardness Condition/form/test basis must match
JIS G4401 SK140 Tool Steel Plate Carbon tool steel; published C 1.30–1.50 % JIS G4401:2009 plate/strip condition basis; as-hot-rolled unless otherwise specified Not the ISO 4957:1999 Table 2/4 specimen test Compare actual carbon, Si/Mn limits, condition and plate rules
JIS G4401 SK120 Tool Steel Plate Carbon tool steel; published C 1.15–1.25 % JIS G4401:2009 plate/strip condition basis; as-hot-rolled unless otherwise specified Not the ISO 4957:1999 Table 2/4 specimen test Compare actual carbon, Si/Mn limits, condition and plate rules
ASTM A829 4140 Alloy Steel Plate Engineering Cr-Mo plate; published C 0.36–0.44 % Ordered condition on the own live page Chemistry-ordered engineering plate, not this tool-test acceptance Not a direct tool-grade substitute

Country comparisons and substitution limits for C45U

The country comparison uses actual cited editions, not an unrestricted trade-name list. The steel number is the informative Annex C designation association, not proof that foreign delivery and test requirements are identical.

System Grade / number Actual chemistry / form difference Condition / substitution limit
ISO / international C45U Cast-analysis Table 2; this grade and edition Delivery condition, specimen response and plate/flat requirements must be specified
Europe / designation number 1.1730 Informative Annex C associates the EN 10027-2:1992 number; it is not an independently verified later DIN specification No automatic national-edition or product-condition certification inferred
United States ASTM A681-08 L2 ASTM C 0.45–1.00 with required Cr 0.70–1.20 and V 0.10–0.30 differs from non-alloy C45U C 0.42–0.50 and its unquoted-alloy rule. Special-purpose tool contrast only, not a C45U counterpart; no exact national equivalent is asserted.

The ISO hardening-test HRC is a genuine specimen-response basis. It must not be confused with JIS G4404 practical-decarburization HV criteria, JIS plate delivery hardness or an informative tempering curve. Verify the complete foreign standard, form and ordered condition before substitution.

Why choose SHH STEEL for C45U

SHH STEEL produces and exports C45U plate against the stated standard, supplied condition and agreed inspection plan. We keep cast analysis, delivery hardness and final tooling acceptance distinct.

  • Confirm the required edition and correct material designation.
  • Use plate/flat tolerances and cleanup allowance appropriate to the actual form.
  • Agree supplementary verification and required reports before acceptance.
  • Maintain heat identification and review any proposed foreign substitution.

Enquiry and inspection planning for C45U

Enquiry item What to specify
Grade / edition C45U; ISO edition and any associated drawing requirement
Form / dimensions Plate or flat, thickness × width × length, quantity, finish and machining allowance
Condition Non-heat-treated (+U); Table 2 footnote c
Hardness basis 207 HB maximum; Table 2 entry bears the untreated-use footnote c, not an annealed-default claim
Verification State whether Annex B.3 hardening verification, product analysis or other supplementary tests are required
Final tooling Actual tool duty, final property acceptance and production-treatment responsibility
Reports / logistics Inspection-document type, heat traceability, packing, destination and target timing

Dimensions, manufacturing route and any additional NDT or quality requirement are reviewed for feasibility. This page is not an unconditional stock, capacity or finished-tool performance commitment.

FAQ

What distinguishes C45U?
The non-heat-treated delivery route distinguishes it from the higher-carbon water-hardening grades; do not assume an annealed default. Its carbon window and untreated-use note do not make it a replacement for high-carbon cutting tools.
Does the HRC value describe supplied plate?
No. The reference hardening test gives 54 HRC minimum on its stipulated specimen basis. The delivery-condition entry is 207 HB maximum; Table 2 entry bears the untreated-use footnote c, not an annealed-default claim. Final tool properties require a separate qualified basis.
Are these temperatures a production heat-treatment guarantee?
No. The table/B.3 regime is a specimen test. Table 1 note c provides the minimum-response requirement, while Annex B.1 makes supplementary verification an enquiry/order item. Annex A curves are informative; actual tool treatment depends on section and application.
Can round hardenability or bar tolerances be used directly for plate?
No. Follow the actual product-form agreement under clause 4.4 and Figure 1 sample rules. Any Table 2 round-diameter hardenability statements are not plate-thickness guarantees.
Is the foreign grade or steel number an automatic equivalent?
No. Use the explicit country-table differences, complete source edition, actual form, delivery condition and test acceptance. Historical JIS names and informative steel-number associations do not establish unconditional substitution.

Request a quotation

Request a quotation for ISO 4957 C45U tool steel plate or flat stock. Send the required edition, quantity, dimensions, finish, machining allowance and drawing. State the supplied condition explicitly: Non-heat-treated (+U); Table 2 footnote c. Identify the intended tooling duty and whether dimensions describe raw blanks or finished pieces.

Include the delivery-hardness acceptance, required inspection document and heat-traceability needs. Specify any supplementary product analysis, Annex B.3 hardening-test verification, surface/decarburization evaluation or additional NDT, with the agreed method and acceptance criteria. Do not treat a specimen-response HRC or round-diameter hardenability note as an arbitrary-section plate guarantee.

Provide the final tool properties and production-treatment responsibility separately. For a proposed foreign grade, attach its governing specification and drawing so chemistry, form and condition differences can be reviewed. Include cutting details, edge preparation, inspection stages, destination, packing and target timing; requested processes and dimensions are reviewed for feasibility before confirmation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X