ISO 2037 316 Stainless Steel Tube

ISO 2037 316 stainless steel tube adds 2–3 % molybdenum for salty and acidic food service, made seamless (TS 60) or welded (TW 60) to ISO 2037 sizes and roughness limits. SHH STEEL can make and supply it for lines, heat exchangers and food equipment.
Grade
316 (commercial) — ISO 2037 steel type TS 60 seamless / TW 60 welded
Standard
ISO 2037:1992 Stainless steel tubes for the food industry (withdrawn 2022, still cited)
Product form
Seamless (TS 60, ISO 2604-2) and welded (TW 60, ISO 2604-5) hygienic tube, straight lengths
Size
OD 12–406.4 mm, wall 1.0–3.2 mm per ISO 2037 Table 1; OD tol. ISO 5252 D4 (≤101.6) / D3, wall T3
Surface
Ra ≤ 1 µm finely finished / Ra ≤ 2.5 µm other; BA, polished or electropolished
Share:
Overview
Chemical Composition
Mechanical Properties
Tube Manufacture
Specification
Equivalent Grades
Heat Treatment
Corrosion Resistance
Applications
Weldability
Surface Finishes
Inspection and Testing
Packaging and Shipping
Why Choose SHH STEEL
Supply Capability
FAQ
Conclusion

What is ISO 2037 316 Stainless Steel Tube

ISO 2037 316 stainless steel tube is food-industry tube built to the dimensional, tolerance, roughness and hygiene rules of ISO 2037:1992 in the standard-carbon chromium-nickel-molybdenum grade. The standard itself calls this steel type TS 60 when the tube is seamless (ISO 2604-2) and TW 60 when it is welded (ISO 2604-5). In the trade it is simply ordered as 316, roughly the X5CrNiMo17-12-2 family with about 2 – 3 % molybdenum.

SHH STEEL can produce and supply ISO 2037 316 tube as seamless TS 60 or as welded and bright-annealed TW 60, polished inside to the Ra limit your line needs. Customers usually come to 316 because 304L has started to pit in salty or acidic service, or because the tube will be formed and used without many site welds and they want the slightly higher strength of the standard-carbon grade.

Grade 316 occupies the middle position in the ISO 2037 range. It has the molybdenum benefit of 316L but carries up to 0.08 % carbon, so it suits factory-built skids, heat exchanger tube bundles and formed components that are annealed after fabrication, rather than long field-welded lines where 316L is the safer choice.

Beside this 316 page, keep tubular RFQs under Stainless Steel Pipes and Tubes, flat RFQs under Stainless Steel Sheets and Plates, and pin the plate twin with ASTM A240 Type 316. Confirm 316 OD × wall and plate thickness on separate drawings.

Chemical Composition of ISO 2037 316 Stainless Steel Tube

ISO 2037 references TS 60/TW 60 through ISO 2604 rather than printing an analysis. For enquiry clarity, the commercial 316 limits from ASTM A269 / A312 are given below; the original ISO 2604 band governs if the purchase order calls for it.

Element 316 commercial limit (wt %)
C ≤ 0.08
Mn ≤ 2.00
P ≤ 0.045
S ≤ 0.030
Si ≤ 1.00
Cr 16.0 – 18.0
Ni 10.0 – 14.0
Mo 2.00 – 3.00

Molybdenum is the element that sets 316 apart from the 304 family. It strengthens the passive film against chloride attack and raises pitting resistance noticeably. Nickel is raised to around 10 – 14 % to keep the structure fully austenitic when chromium is lowered to 16 – 18 %, which also gives 316 good toughness and formability.

The higher carbon allowance, up to 0.08 %, is the trade-off. It gives a little more strength but makes the grade sensitive to carbide precipitation if welds are held in the 450 – 850 °C range, which is discussed under weldability.

Mechanical Properties of ISO 2037 316 Stainless Steel Tube

Mechanical acceptance under ISO 2037 follows the referenced material standard. The commercial 316 tube minimums most engineers work with are shown here; they are higher than those of 304L and 316L because of the extra carbon.

Property 316 commercial minimum
Tensile strength Rm 515 MPa
Yield strength Rp0.2 205 MPa
Elongation A 35 %
Hardness (A269 max) 90 HRB

The roughly 35 MPa higher proof strength against 316L allows slightly higher design pressure at the same thin wall, which is useful on heat exchanger tubes, homogeniser feed lines and pressurised UHT sections. For standard CIP and product transfer at a few bar, the difference rarely controls the wall thickness, which is fixed by Table 1 anyway.

Tube Manufacture of ISO 2037 316: Seamless TS and Welded TW Routes

For 316 the seamless TS 60 route is common because many 316 food tubes end up in heat exchangers, coils and machined parts. Billets of 316 are hot-extruded or rotary pierced, then cold-pilgered and cold-drawn in several passes with intermediate anneals. The finished tube is solution annealed and rapidly cooled, which also redissolves carbides so the higher-carbon grade leaves the mill fully corrosion resistant.

The welded TW 60 route uses 316 cold-rolled strip formed and fused by TIG, plasma or laser without filler. Molybdenum-bearing melts are a little more viscous, so mills tune welding speed and shielding to get a flush bead. Bead-rolling, bright annealing and sizing follow. For welded 316 the in-line anneal is essential, as it removes any carbides formed in the seam heat-affected zone.

We advise customers on route choice based on wall and end use: welded 316 for straight lines and frames, seamless 316 for coils, bent heat-transfer tube and thicker walls where a homogeneous structure is preferred.

Dimensions and Tolerances for ISO 2037 316 Tube

The preferred sizes for ISO 2037 316 tube are the same as for every grade in the standard, taken from ISO 1127 series 1 and 2. The table below lists each outside diameter with its wall, followed by the tolerance and roughness clauses that apply.

OD (mm) Wall (mm) OD (mm) Wall (mm)
12 1.0 76.1 1.6
12.7 1.0 88.9 2.0
17.2 1.0 101.6 2.0
21.3 1.0 114.3 2.0
25 1.2 / 1.6 139.7 2.0
33.7 1.2 / 1.6 168.3 2.6
38 1.2 / 1.6 219.1 2.6
40 1.2 / 1.6 273 2.6
51 1.2 / 1.6 323.9 2.6
63.5 1.6 355.6 2.6
70 1.6 406.4 3.2
Item ISO 2037:1992 clause Requirement
OD ≤ 101.6 mm 4.1 ISO 5252 class D4
OD > 101.6 mm 4.1 ISO 5252 class D3
Wall thickness 4.2 ISO 5252 class T3
Finely finished surface 5.1 Ra ≤ 1 µm
Other surfaces 5.2 Ra ≤ 2.5 µm
Welded seam 5.2 not to exceed 16 µm (see flag)

In 316 we see more demand for the heavier walls, such as 88.9 × 2.0, 114.3 × 2.0 and 168.3 × 2.6 mm, because 316 is often used in equipment builders’ shops for vessels nozzles and heat exchanger shells. Class D4 OD tolerance below 101.6 mm keeps the tube suitable for tube-sheet expansion as well as orbital welding.

Standard length is 6 m; fixed lengths for exchanger bundles and U-bends are produced on order. Where equipment combines ISO and inch-series sanitary tube, we can also supply 316 in OD 1” to 4” sanitary sizes alongside the ISO 2037 range.

Equivalent Grades for ISO 2037 316

Cross-references for ISO 2037 316 are chemistry-family guides for enquiry, not automatic dual certification. Compare ISO 2037 316L for the low-carbon version and ISO 2037 304L for the molybdenum-free grade. Lock 316 on the purchase order when the food-tube drawing needs molybdenum-bearing austenitic chemistry under ISO 2037.

System Designation Notes
ISO 2037 seamless TS 60 (ISO 2604-2) Governing seamless food-tube route for this page when ordered seamless
ISO 2037 welded TW 60 (ISO 2604-5) Governing welded food-tube route under ISO 2037
Commercial / UNS (body only) 316 / UNS S31600 Useful in dual-cert talk; not a substitute on the PO/MTC by itself
ASTM A269 / A270 related TP316 family Related chemistry — different product standard; not interchangeable by default
EN / other 1.4401 (X5CrNiMo17-12-2) Starting point for comparison only; order EN product under the EN tube spec
JIS SUS316 Approximate Japanese grade name; confirm the Japanese tube product standard

Related live pages include ASTM A269 TP316, ASTM A312 TP316 and EN 10216-5 1.4401. The TS 60 to 316 mapping is the most consistent of the three ISO 2037 grades across reference sources, but many mills now supply dual-certified 316/316L, so check which carbon limit the drawing needs. Hub: ISO 2037.

Heat Treatment and Delivery Condition for ISO 2037 316

ISO 2037 316 tube is supplied solution annealed, typically from about 1040 °C upward with rapid water or gas cooling. This step matters more for 316 than for the L grades because the higher carbon will form chromium carbides if the tube is cooled slowly or held in the sensitising range. Correct annealing leaves a uniform austenitic structure with all carbon in solution.

Welded 316 is usually bright annealed in hydrogen in-line, which gives a clean reflective surface ready for polishing. Seamless 316 is furnace annealed, then pickled and passivated. For parts that will be heavily formed, such as coils or flared tube, we can supply a softer anneal condition on request.

Unlike 304L and 316L, fabricated 316 assemblies with substantial welding are best re-annealed or at least pickled and passivated, so that weld-zone corrosion resistance matches the parent tube. This is why 316 is preferred for shop-made equipment.

Corrosion Resistance of ISO 2037 316 Tube

Molybdenum makes 316 considerably better than 304L in chloride-bearing food media. It handles brine, salted dairy products, ketchup, mustard, vinegar, fruit juices with higher acidity and seawater-based cooling better, and it tolerates the occasional acid cleaning cycle with nitric or phosphoric acid. Pitting resistance equivalent (PREN) is several points above that of 304L.

The limit is intergranular corrosion after welding. If welded joints are left unannealed and later exposed to acid cleaning or hot chloride solutions, carbide-depleted zones can corrode. For long site-welded lines in such service, the low-carbon 316L is the better choice; for equipment that is annealed or welded with low heat input, 316 performs well.

Like all austenitic grades, 316 can still crack under combined chloride, tensile stress and temperature above about 60 °C, so hot brine heat exchangers need careful design and cleaning procedures.

Applications of ISO 2037 316 Tube in Food, Dairy and Beverage Lines

ISO 2037 316 tube is used where the product is salty or acidic and the components are built in a shop: tubular heat exchangers for sauces and juices, pasteurisers and UHT heaters, cheese brine systems, pickle and vinegar lines, and process equipment frames in wet, salty washdown areas such as fish and meat processing.

Beverage plants use 316 for syrup and concentrate handling, carbonation systems and acidic juice lines. In pharma-adjacent hygienic plants it appears in equipment for nutraceuticals and food additives, though purified water and injectables lines nearly always specify 316L. Equipment builders also choose 316 for its strength in coil and spiral heat-transfer tube.

The common factor is that the tube needs better chloride resistance than 304L while being formed or annealed under controlled conditions, rather than welded in the field. Typical buyers are OEMs of pasteurisers and sauce cookers rather than end users installing long pipe runs.

Weldability of ISO 2037 316 Tube

316 welds readily by TIG, plasma and laser processes. Thin hygienic walls are usually welded autogenously with orbital equipment and full argon purge; with filler, ER316L is preferred over ER316 so that the weld metal itself is low carbon. Low heat input and fast travel keep time in the sensitising range short.

Because base metal carbon can reach 0.08 %, a weld HAZ in 316 can sensitise if multiple passes or slow cooling occur. Good practice is to restrict interpass temperature to about 150 °C, avoid unnecessary repairs, and pickle and passivate or anneal fabricated assemblies before product contact.

For projects that will be site-welded in quantity, we usually recommend dual-certified 316/316L or straight 316L, which gives the same molybdenum benefit with no HAZ sensitisation risk. Where an assembly cannot be annealed, a pickling paste treatment of the weld zone followed by rinse and passivation restores most of the lost resistance.

Surface Finishes for ISO 2037 316 Tube

ISO 2037 clause 5 sets Ra ≤ 1 µm for finely finished surfaces and Ra ≤ 2.5 µm for other surfaces, with a separate weld-seam limit. 316 tube for food contact is normally ordered with inside Ra ≤ 0.8 µm, either by mechanical polish or bright annealing, and outside polish for appearance and cleanability. Because 316 takes mechanical and electrolytic polish well, finish scope (OD versus ID) should be as explicit as the molybdenum line on the order.

Finish Typical supply Order note
Bright annealed (ID/OD) Common for heat-exchanger and food bore without abrasion marks State OD, ID, or both
Internal mechanical polish Product-contact bore to agreed Ra Name Ra/grit; bore often critical
External satin polish Wipe-down appearance in washdown rooms Name OD scope
Electropolished Salty washdown and low-build-up lines Leaves Cr/Mo-enriched surface; not a substitute for anneal
Passivated When hygienic end-user specs require it Not a substitute for correct heat treatment

Under clause 7 the bore must be clean, smooth and free of inclusions and grooving; visual and borescope checks on each lot support that for 316. Measured inside Ra can be recorded on the certificate so the equipment builder can show compliance. Keep free-iron tooling and chloride-bearing packing films off finished food tube before shipment.

Inspection and Testing for ISO 2037 316 Tube

Testing of ISO 2037 316 tube combines the dimensional and roughness checks of the standard with the material tests of ISO 2604. Each lot is inspected for OD, wall, straightness and length, and roughness is measured with a stylus profilometer. Welded TW 60 tube is eddy-current tested along the full length and checked by flattening and flare tests on the seam.

Seamless TS 60 tube receives flattening, flaring and hydrostatic or eddy-current testing. PMI on every bundle confirms molybdenum, which is essential because 316 and 304 look identical. Intergranular corrosion testing to ISO 3651-2 or ASTM A262 Practice E can be added on request to prove correct solution annealing.

Results are documented on EN 10204 3.1 certificates as standard or 3.2 with third-party inspection, showing the ISO 2037 type and the commercial grade 316.

Packaging and Shipping for ISO 2037 316 Tube

316 tube is protected with end caps and plastic sleeves and bundled in hexagonal form, with stainless or nylon strapping and no direct contact with carbon steel. Polished or electropolished lengths are packed individually in PE film and then boxed in plywood crates with moisture barrier.

Each bundle is labelled with the standard, grade 316, TS 60 or TW 60 route, size, length and heat number; the tube itself is ink-jet marked along its length. Exchanger tubes and U-bends are packed in custom crates with spacers to protect bends. Shipping is by FCL, LCL or air depending on urgency.

Why Choose SHH STEEL

SHH STEEL can make and supply ISO 2037 316 tube for equipment builders as well as plant owners. We hold seamless TS 60 and welded TW 60 stock, produce heat-exchanger lengths and U-bends, and give honest advice on whether 316, 316L or dual certification fits your fabrication method.

Every lot is PMI-checked for molybdenum, every bore is roughness tested, and we can add intergranular corrosion testing when the duty involves acid cleaning. With polishing, cutting and packing done in-house, we deliver consistent, traceable tube for food and beverage equipment. We also tell you plainly when 316 is not the right answer and a 316L or dual-certified tube will save trouble on site.

Supply Capability

SHH STEEL can supply ISO 2037 316 tube across the Table 1 range from 12 to 406.4 mm OD. Stock / Available sizes: 25 × 1.6, 38 × 1.6, 51 × 1.6, 63.5 × 1.6, 76.1 × 1.6, 88.9 × 2.0, 101.6 × 2.0, 114.3 × 2.0 and 168.3 × 2.6 mm, seamless and welded, bright annealed or polished, mostly in 6 m lengths.

Fixed exchanger lengths, coils and U-bends are made on order, usually within four to eight weeks. Smaller diameters from 12 to 21.3 mm are available as seamless tube for instrument and heat-transfer duty. See the ISO 2037 hub for all three grades.

FAQ

What is ISO 2037 316 stainless steel tube?
It is food-industry tube made to ISO 2037:1992 sizes, tolerances and surface roughness, in the molybdenum-bearing 316 grade. The standard lists the steel type as TS 60 for seamless tube (ISO 2604-2) and TW 60 for welded tube (ISO 2604-5). It suits salty and acidic food duty where 304L would pit.
How does ISO 2037 316 differ from 304L?
316 contains 2 – 3 % molybdenum and more nickel, which gives much better resistance to chloride pitting and crevice corrosion in salty or acidic foods. 304L has no molybdenum but lower carbon, so it is cheaper and very easy to weld for mild service. The price premium over 304L is usually repaid by longer service life in those products.
How does ISO 2037 316 differ from 316L?
Both contain the same molybdenum, but 316 allows up to 0.08 % carbon while ISO 2037 316L is limited to 0.035 % or less. 316 is slightly stronger; 316L is safer for heavily site-welded lines because it does not sensitise next to the weld. Many projects therefore buy dual-certified 316/316L to keep both options open.
Is TS 60 the same as AISI 316?
Most reference sources map TS 60 to 316, close to EN 1.4401. It is the most consistent mapping in the ISO 2037 range, but the original ISO 2604-2 chemistry governs if your contract names TS 60, so state both the ISO type and 316 on the order. Our certificates show both designations side by side when requested.
Can ISO 2037 316 tube be welded on site?
Yes, but take care. Use low heat input, argon back-purge and ER316L filler where filler is required, keep interpass temperature low, and pickle and passivate afterwards. For long site-welded lines in aggressive service, 316L or dual-certified 316/316L is usually recommended. Mills can certify both if the heat meets the tighter carbon limit.
What sizes are available in ISO 2037 316?
ISO 2037 Table 1 covers 12 × 1.0 mm through 406.4 × 3.2 mm. For 316 we most often supply 38 to 168.3 mm OD with 1.6 to 2.6 mm wall, plus small seamless sizes for heat-transfer coils and instrumentation. Larger diameters up to 406.4 × 3.2 mm are produced on order, normally as welded tube.
What is the minimum strength of 316 tube?
Commercial 316 tube is normally certified to at least 515 MPa tensile strength, 205 MPa yield strength and 35 % elongation, as in ASTM A269. ISO 2037 itself sets no tensile values; they come from the referenced material standard. Tensile, flattening and flare results are reported on the 3.1 certificate for each heat and lot.
Which foods require 316 instead of 304L?
Products with salt or acids such as brine, cheese whey, sauces, ketchup, pickles, vinegar and some fruit juices, and washdown areas in fish and meat plants. In these environments 304L can pit, while the molybdenum in 316 keeps the passive film stable. Fish, meat and cheese processing areas with salty washdown are typical examples where we recommend 316.
What surface finish is supplied on ISO 2037 316 tube?
The standard requires Ra ≤ 1 µm on finely finished surfaces and Ra ≤ 2.5 µm elsewhere. We normally supply Ra ≤ 0.8 µm inside, by bright annealing or mechanical polish, and offer electropolishing for demanding hygienic or salty applications. Outside surfaces are normally satin polished for appearance and easy wipe-down in food plants.
Can intergranular corrosion testing be done on 316 tube?
Yes. Because 316 has higher carbon, owners sometimes request intergranular corrosion testing to ISO 3651-2 or ASTM A262 Practice E. It proves that the tube was properly solution annealed and is free from harmful carbides before installation. It is most useful after welded or formed fabrication where the anneal history is uncertain.
Does SHH STEEL supply ISO 2037 316 heat exchanger tube?
Yes. SHH STEEL can supply ISO 2037 316 tube in fixed lengths, coils and U-bends for tubular heat exchangers and pasteurisers, with exchanger-grade OD tolerance, hydrostatic or eddy-current testing and full traceability. Bundles are packed in custom crates to protect bends during transport.

Conclusion

ISO 2037 316 stainless steel tube gives food and beverage equipment molybdenum-level chloride resistance with slightly higher strength than the L grades, available as seamless TS 60 or welded TW 60. SHH STEEL can make and supply it from stock and to order, including exchanger lengths and U-bends. For heavily site-welded lines see ISO 2037 316L; for mild service compare ISO 2037 304L and ASTM A269 TP316. Email admin@steelspecs.com for a quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response