GB/T 4238 20Cr25Ni20 S31020 Heat Resistant Steel Plate
What is GB/T 4238 20Cr25Ni20 S31020 Heat Resistant Steel Plate?
Equivalent grades: 20Cr25Ni20 (S31020) ≈ UNS S31000 ≈ JIS SUH310 ≈ EN 1.4845 X8CrNi25-21 (nearest).
20Cr25Ni20 (S31020) is a heat-resistant grade. 20Cr25Ni20 is the Chinese 310 heat-resistant grade with up to 0.25 % carbon. It resists oxidation to about 1100 °C and is used for furnace parts that see high temperature and some load.
GB/T 4238-2015 is the Chinese national standard for heat-resisting steel plate and strip. It lists austenitic, ferritic, martensitic and precipitation-hardening grades chosen for oxidation resistance and strength at high temperature, and it is the GB equivalent of EN 10095 and JIS G4312 for furnace and boiler plate.
This page sets out the GB/T 4238-2015 requirements for 20Cr25Ni20 (S31020) plate: specification summary, chemistry, mechanical properties, high-temperature behaviour, heat treatment, finishes and tolerances, current stock, equivalents, fabrication and testing. SHH STEEL supplies it mill-direct from China with EN 10204 3.1 certificates, optional third-party inspection and in-house cutting.
20Cr25Ni20 (S31020) plate: specification summary
| Item | 20Cr25Ni20 (S31020) data |
|---|---|
| Standard | GB/T 4238-2015, heat-resisting steel plate and strip |
| Product forms | hot-rolled and cold-rolled plate, sheet and strip |
| Typical thickness | 3–80 mm hot-rolled plate; 0.5–6 mm cold rolled |
| Widths | 1500, 1800, 2000 mm |
| Lengths | 6000 mm or cut to size |
| Finishes | No.1 (hot rolled, annealed, pickled); 2D/2B for cold rolled |
| Heat treatment | solution treated (austenitic) or annealed (ferritic) |
| Tests | chemical analysis, tensile, hardness |
| Certificates | mill certificate to GB/T 18253 (EN 10204 3.1 type); 3.2 on request |
| Grade family | heat-resistant |
Size range. Plate is produced on Steckel or reversing mills from about 5 mm up to 80–100 mm depending on grade, with widths of 1500–2500 mm and lengths up to 12 m; thinner plate of 3–12 mm is often cut from hot-rolled coil. Very heavy or wide plates, and plates with tight flatness, should be confirmed before ordering. 20Cr25Ni20 (S31020) is produced regularly by several mills; common sizes are held in stock, and other sizes are rolled in the mill’s scheduled campaigns for the grade.
Chemical composition of 20Cr25Ni20 (S31020) (GB/T 4238-2015)
| Element | wt % |
|---|---|
| C | 0.25 max |
| Si | 1.50 max |
| Mn | 2.00 max |
| P | 0.040 max |
| S | 0.030 max |
| Cr | 24.00–26.00 |
| Ni | 19.00–22.00 |
Single values are maximums unless marked min. Ranges are heat (cast) analysis limits.
For heat-resistant grades the key elements are chromium (oxide scale), nickel (austenite stability, carburisation resistance) and silicon, aluminium or rare earths where present (scale adhesion). Sulfur and phosphorus are kept low to protect hot ductility and weldability.
Mechanical properties of 20Cr25Ni20 (S31020) plate
| Rp0.2 min, MPa | Rm min, MPa | A min, % | HBW max | HRB max | HV max |
|---|---|---|---|---|---|
| 205 | 515 | 40 | 217 | 95 | 220 |
The minimum proof strength is 205 MPa. For high-temperature design, room-temperature values are only an acceptance check; use creep and stress-rupture data from the standard’s informative annexes or the ASME allowable stresses where Code rules apply. Tension tests are taken in the direction stated in the standard; where a hardness limit is given, it is a maximum that confirms correct annealing.
High-temperature behaviour of 20Cr25Ni20 (S31020)
This is a heat-resistant grade: it is selected for oxidation resistance, strength and structural stability at high temperature rather than for wet corrosion. Chromium forms the protective oxide, nickel stabilises the austenite against thermal cycling and carburisation, and silicon, rare earths or nitrogen, where present, improve scale adhesion or creep strength. The maximum useful temperature in air depends on atmosphere, thermal cycling and load, so published scaling temperatures are a guide, not a design value.
Sulfur-bearing gases attack high-nickel alloys, while carburising or nitriding atmospheres favour higher nickel; vanadium-bearing ash and molten salts need special evaluation. Long exposure in the 600–900 °C range can form sigma phase in high-chromium grades and reduce room-temperature toughness, which matters for parts that are cleaned or repaired cold. Creep-rupture values are given in the standard’s informative annexes or by the mill and should be used for design instead of room-temperature strength.
How 20Cr25Ni20 (S31020) compares with related grades
| Grade | Cr | Ni | Mo | N | PREN (min) | YS / Rp0.2 min, MPa |
|---|---|---|---|---|---|---|
| 20Cr25Ni20 (S31020) | 24.00–26.00 | 19.00–22.00 | — | — | — | 205 |
| 16Cr23Ni13 (S30920) | 22.00–24.00 | 12.00–15.00 | — | — | — | 205 |
| 06Cr23Ni13 (S30908) | 22–24 | 12–15 | — | — | — | 205 |
| 06Cr25Ni20 (S31008) | 24–26 | 19–22 | — | — | — | 205 |
| 08Cr21Ni11Si2CeN (S30859) | 20–22 | 10–12 | — | 0.14–0.2 | — | 310 |
Choose 20Cr25Ni20 (S31020) when oxidation resistance and strength at temperature drive the selection. For wet corrosion at room temperature, a low-carbon corrosion-resistant grade is usually a better choice, and in sulfur-rich gases a lower-nickel grade may outperform a high-nickel one.
The table uses specification limits, not typical mill values, so it shows the guaranteed position of each grade. Final selection should also consider product availability in the thickness you need, welding consumables, and the inspection requirements of your project.
Heat treatment and delivery condition of 20Cr25Ni20 (S31020)
Heat treatment: 1030–1180 °C, rapid cooling.
Heat-resistant plate is supplied solution annealed. For high-temperature service, a coarser grain size improves creep strength, while a finer grain improves fatigue and room-temperature ductility; where it matters, state the grain-size requirement on the order. Stress relief is not normally needed.
Surface finishes for 20Cr25Ni20 (S31020) plate
Hot-rolled plate to GB/T 4238 is normally supplied solution treated and pickled (No.1). Thin cold-rolled sheet comes in 2D or 2B. For furnace use the finish is less important than flatness and edge condition.
Dimensions, tolerances and flatness
Dimensional tolerances refer to GB/T 709 for hot-rolled plate and GB/T 708 for cold-rolled sheet, unless the order states otherwise. Ordered thickness, width and flatness class should be on the contract.
Chinese grade names and codes. GB/T 4238 uses the GB/T 20878 grade names and unified numeric codes (ISC) such as S31020. A plate that is certified to GB/T 4237 is not automatically acceptable for GB/T 4238 service, because the heat-resisting standard has its own grade list and property requirements. Order with the grade name and code, the delivery condition, the thickness tolerance class and the certificate type; for boiler or pressure parts, also state the applicable pressure-equipment rules.
20Cr25Ni20 (S31020) plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Finish | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1500 / 2000 | 6000 | No.1 | 200+ t | China |
| 8 | 1500 / 2000 | 6000 | No.1 | 200+ t | China |
| 10 | 2000 | 6000 | No.1 | 100+ t | China |
| 12 | 2000 | 6000 | No.1 | 100+ t | China |
| 16 | 2000 / 2500 | 6000 | No.1 | 100+ t | China |
| 20 | 2000 / 2500 | 6000 / 8000 | No.1 | 100+ t | China |
| 30 | 2000 / 2500 | 6000 | No.1 | 100+ t | China |
Quantities are approximate and stock changes daily. Send your size list for current availability; other thicknesses, widths and cut sizes can be supplied from mill production.
Packing and logistics. Plate is bundled on steel or wooden skids with steel bands and edge protection, typically 3–8 t per bundle, and marked with heat and plate numbers. Cut pieces are crated. Heavy and wide plate ships in open-top or flat-rack containers or by break-bulk; we send loading photos with the shipping documents.
20Cr25Ni20 (S31020) equivalents in other standards
| Standard | Designation | Comment |
|---|---|---|
| ASTM / UNS | UNS S31000 | same alloy family and limits closely matched; compare each limit on the certificate |
| JIS | SUH310 | same alloy family and limits closely matched; compare each limit on the certificate |
| EN | 1.4845 X8CrNi25-21 | nearest grade only; limits differ, check before substituting |
Equivalents are close, not identical. When a project names one standard, order to that standard or ask for multiple certification and check every limit on the certificate.
Related grades by alloy family
Same standard
Other grades in this standard: GB/T 4237 S30908, GB/T 4237 S31008, GB/T 4237 S30859, GB/T 4238 S30920, GB/T 4238 S30908, GB/T 4238 S31008.
Heat-resistant
Heat-resistant grades ranked by chromium, nickel and silicon: A240 S30908, A240 S31008, A240 S30909, A240 S31009, 1.4948 (EN 10028-7), 1.4950 (EN 10028-7).
Applications, forming and welding of 20Cr25Ni20 (S31020)
Typical uses: furnace muffles, radiant tubes, burner nozzles and kiln parts.
Heat-resistant plate is usually cut by plasma or waterjet, formed hot or cold, and welded with matching heat-resistant consumables. Cut by plasma, laser or waterjet and remove heat tint by pickling or grinding. For welding use a matching heat-resistant filler such as ER309, ER310 or ERNiCr-3 according to the service temperature. Keep the weld area clean and free of carbon-steel contamination, and pickle and passivate after welding where corrosion resistance matters.
Fabrication at temperature. Design furnace parts to allow for thermal expansion, which is about 1.5 times that of carbon steel, and avoid sharp corners where scale can spall. Welds should be full penetration where they carry load at temperature. For high-silicon grades, use low heat input to limit hot cracking. After long service, high-chromium plate may be embrittled by sigma phase, so repair welding of old parts needs care and sometimes a solution anneal first.
Certificates, testing and receiving inspection
Every delivery carries a mill certificate to GB/T 4238-2015 with heat analysis, tensile results and hardness, and the grade and standard as ordered. Supplementary tests we can arrange: PMI, grain-size measurement (ASTM E112) where the grade requires it, elevated-temperature tensile tests by agreement, and ultrasonic testing of heavy plate. Third-party witness by SGS, BV, TÜV, DNV, ABS or LR is available with EN 10204 3.2 certificates.
On receipt, check marking and heat number against the certificate, measure thickness at several points and confirm the finish and edge condition before cutting.
Common mistakes when specifying 20Cr25Ni20 (S31020)
- Selecting by room-temperature strength instead of creep data.
- Substituting a low-carbon corrosion grade (for example 310S for 310) without checking creep strength.
- Ignoring the atmosphere: sulfur, carburising gas and vanadium ash change the ranking of grades.
Each of these can be avoided by writing the requirement into the purchase order and checking it on the certificate before the material is cut.
Sourcing 20Cr25Ni20 (S31020): buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Wrong grade substitution (for example 304 for 309/310) | PMI of every plate before dispatch |
| Distortion of large furnace panels | levelled plate and cut-to-size blanks with low-stress cutting |
| Small quantities across many sizes | mixed thicknesses and grades combined in one shipment |
| Cutting and edge preparation | in-house shearing, plasma, laser and waterjet cutting, bevelling |
| Delivery delays | weekly production and shipping updates with photos |
How to order 20Cr25Ni20 (S31020) plate
State the standard and edition (GB/T 4238-2015), the grade (20Cr25Ni20 (S31020)), thickness, width and length or coil, finish, quantity, tolerance class, any added chemistry limits, the supplementary tests and acceptance values from your specification, the certificate type and inspection agency, and packing. Send the list to SHH STEEL and we will reply with price, available stock and lead time.
FAQ
-
When should I order GB/T 4238 instead of GB/T 4237?
- Order GB/T 4238 when the plate is for high-temperature service such as furnaces, boilers and heat-treatment equipment. GB/T 4237 is for general corrosion-resistant use.
-
Is 20Cr25Ni20 (S31020) equivalent to UNS S31000?
- They are the same alloy designation in different standards. Limits are closely matched, but always order to the standard named in your specification or ask for multiple certification.
-
What is the maximum service temperature of 20Cr25Ni20 (S31020)?
- It depends on the atmosphere, thermal cycling and load. Published scaling temperatures are a guide for oxidation in air only; for load-bearing parts use creep-rupture data.
-
Can I order small quantities or cut sizes?
- Yes. We combine mixed thicknesses and grades into one shipment and cut plate and sheet to size in our workshop.
-
Which certificates and tests can you provide?
- Every order ships with a mill certificate (EN 10204 3.1 type) showing heat analysis and mechanical tests. Supplementary tests and 3.2 certificates with SGS, BV, TÜV or another agency are available by agreement.
Conclusion
20Cr25Ni20 (S31020) plate should be ordered with the points the standard leaves open written into the contract: finish, tolerance class, any extra chemistry limits and the supplementary tests your application needs. With those fixed, stock material from China is a fast and reliable route.