GB/T 1299 9SiCr Tool Steel Plate | GB/T 1299 Tool Steel - SHH STEEL

GB/T 1299 9SiCr Tool Steel Plate

GB/T 1299 9SiCr is a silicon-chromium measuring and cutting tool steel for measuring tools, cutting blanks and supported precision tooling. This page uses the finalized historical alloy tool steel edition, not an unverified current chemistry table. Plate enquiries need an explicit product form agreement because the cited specification principally covers bar and flat stock. Delivery condition, specimen hardening response and finished tool requirements remain separate acceptance matters. SHH STEEL produces and exports 9SiCr tooling stock against the agreed edition, form and inspection requirements.
Equivalent Grades:
Country differences require full-source review; no automatic equivalent.
Heat Treatment
Annealed.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
Conclusion

What is GB/T 1299 9SiCr tooling plate?

GB/T 1299 9SiCr Tool Steel Plate identifies formal grade 9SiCr, unified numeric code T30100, Table 1 row 1-1 of GB/T 1299-2000. Its substantial silicon window distinguishes it from a generic carbon tool steel; the negotiated screw-cutting-tool annealed option must not replace ordinary delivery acceptance.

This is an edition-specific historical technical draft. The officially current standard is GB/T 1299-2025, effective 2026-05-01; its complete chemistry tables have not been verified for this article. Do not treat the historical values below as a current-edition certificate. [S1, S2]

The 2000 scope covers hot-rolled, forged, cold-drawn and bright bars; its chemistry also applies to ingots, billets and products. Hot-rolled and forged flat bars are addressed separately in the dimensional clauses. A commercial plate enquiry therefore needs a stated flat-bar or independently agreed plate acceptance basis: the bar specimen response is not an arbitrary plate-thickness guarantee. [S1 §1, §4]

SHH STEEL produces and exports 9SiCr tooling stock to an agreed specification and documented inspection basis. The existing GB/T 1299 hub is a navigation reference, not a new grade classification.

For plate supply, use this historical grade chemistry together with an expressly agreed product and inspection specification; bar and flat-steel provisions do not automatically establish rolled-plate conformity.

Material specification for 9SiCr

Item Historical source / qualification
Grade / edition 9SiCr; GB/T 1299-2000, Table 1 row 1-1
Unified code T30100; code for this grade, not a separate grade
Source family Measuring and cutting tool steel
Default delivery Annealed under §5.2; do not infer prehardened delivery
Delivery hardness 197–241 HBW 10/3000; Table 3
Specimen response 62 HRC minimum after the source hardening test; not delivery HRC
Form Bar/flat-bar requirements are not automatic rolled-plate acceptance
Edition status Historical 2000 basis; not complete current 2025 requirements

Cast-analysis composition of 9SiCr

Table 1 gives melting/cast-analysis requirements, mass percent. Residual copper and combined copper-plus-nickel requirements are added from §5.1.3, not omitted because their cells are outside the named alloy row. [S1 printed pp3,5]

Element / residual condition Mass %
Carbon (C) 0.85–0.95
Silicon (Si) 1.20–1.60
Manganese (Mn) 0.30–0.60
Phosphorus (P) ≤0.030
Sulfur (S) ≤0.030
Chromium (Cr) 0.95–1.25
Residual copper (Cu) ≤0.30
Residual Cu + Ni ≤0.55

Unquoted alloy cells are not zero-residual guarantees. Product-analysis permissible deviations are referred by §5.1.4 to GB/T 222-1984 Table 2; no unverified numeric deviation is added to these cast-analysis limits. A certificate must identify cast versus product analysis. The special reduced-molybdenum agreement in §5.1.2 applies to 5CrNiMo, not this grade.

Delivery hardness and specimen response for 9SiCr

Delivery hardness and specimen-test response apply in the historical source’s stated product and test context. For plate orders, agree the supplied condition, hardness, dimensions, surface quality, decarburization, sampling and inspection separately; specimen results do not guarantee full-section plate or finished-tool hardness.

The Table 3 delivery requirement is 197–241 HBW 10/3000, and the hardening-test response is at least 62 HRC. The Brinell entry is a range, not merely an annealed maximum; the printed descending endpoints are normalized ascending here.

Acceptance item Requirement / meaning
Supplied annealed stock 197–241 HBW 10/3000
Hardened specimen ≥62 HRC under the source test conditions
Routine test exemption §5.4.1 permits omission of the specimen test where the supplier guarantees conformity; the response requirement remains
Actual finished tool Agreed separately for the real geometry and qualified production process

This is normative historical delivery/response acceptance, not an informative tempering-curve estimate. No tensile strength, impact energy, service temperature or plate-through-hardness is inferred. [S1 §5.4/Table 3]

Only by purchaser/supplier agreement, annealed 9SiCr for screw-cutting tools may use 187–229 HBW 10/3000 under §5.4.2. This is an order-specific use/condition option, not a separate formal grade and not the ordinary 197–241 requirement.

Delivery condition and reference hardening test for 9SiCr

The default delivery state is annealed (§5.2). The expressly permitted prehardened delivery exceptions in that clause are other named grades, not this row. No quality suffix or treatment variant is invented as an additional Table 1 grade.

Table 3 specimen-test item Exact source entry
Hardening temperature 820–860 °C
Quench medium Oil
Minimum response 62 HRC
Row-specific preheat / temper Not printed for this row; none invented
Hardness-test distinction Brinell delivery versus Rockwell hardened specimen

Table 3 note 1 defines holding time after the specimen reaches temperature and distinguishes salt-bath and controlled-atmosphere-furnace cases. These rows do not assign a heating method, so no universal soak or production cycle is inferred. Note 2 addresses the explicitly stated tempering temperatures in other rows; it is not a new tempering recipe for this grade. The printed hardening range and quench are a specimen test, not a qualified treatment schedule for every tool section. [S1 Table 3 and notes, printed pp6–7]

Welding and surface processing 9SiCr

9SiCr is tooling stock rather than a generic weldable structural plate. Repair welding needs a qualified procedure addressing carbon/alloy content, prior treatment, restraint, crack risk and subsequent inspection. No unsupported preheat, interpass or post-weld temperature is prescribed.

Thermal cutting, grinding and EDM may alter the working surface. Specify cleanup allowance, edge preparation and inspection of critical tool features; a conforming heat analysis alone does not prove an undamaged finished edge.

Flat/plate dimensions and surface acceptance

Clauses 4.1–4.5 refer the respective hot-rolled, forged, cold-drawn and flat-bar forms to their named dimensional standards and agreed groups. Clause 4.6 sends other materials/products to the relevant national/industry standard, or supplier/purchaser agreement where none applies. Do not relabel a bar tolerance as a plate tolerance. [S1 printed p2]

Flat-steel surface quality is agreed under §5.8.4. Flat-steel decarburization, and round/side-size stock above 150 mm, are agreement matters under §5.6.1; the round/side-size formulas in Table 5 are not plate-thickness guarantees. Agree flatness, surface, edge quality and cleanup material for the actual form. No unverified plate capacity range or mill stock availability is asserted.

For annealed stock, §5.5.2.1 includes this grade in network-carbide assessment: non-flat cross-section size ≤60 mm has maximum grade 3; flat steel and section size >60 mm require agreement. The tighter grade 2 screw-cutting option applies only to agreed 9SiCr use within the stated section-size qualification, not automatically to plate. Amendment No.1 adds a Table8 note that network-carbide specimen heat treatment follows Table3. [S1 printed p8]

Applications and selection limits for 9SiCr

Qualitative engineering selection for 9SiCr can include measuring tools, cutting blanks and supported precision tooling. Its substantial silicon window distinguishes it from a generic carbon tool steel; the negotiated screw-cutting-tool annealed option must not replace ordinary delivery acceptance. These application suggestions do not add normative tool-life, impact-energy or load ratings to the specification.

Match working-edge support, wear mechanism, section, processing route and inspection to the actual tool. The specified specimen HRC is a material response check; it does not predict distortion or guarantee full-section hardness in a purchased plate blank.

Compare 9SiCr with three live own product pages

These three own product pages were verified live for this batch. They are explicit material-selection contrasts, not unpublished drafts or asserted equivalents.

Published own product Material distinction Acceptance distinction Selection caution
JIS G4401 SK105 Tool Steel Plate Carbon tool steel contrast, not a certified counterpart Published JIS product/condition basis; do not import this GB bar test Review carbon, alloying, supplied condition and actual plate scope
JIS G4401 SK120 Tool Steel Plate Carbon tool steel contrast, not a certified counterpart Published JIS product/condition basis; do not import this GB bar test Review carbon, alloying, supplied condition and actual plate scope
ASTM A829 4140 Alloy Steel Plate Engineering alloy plate contrast Chemistry-ordered plate, not this tool-steel specimen acceptance A readily compared plate page is not substitution approval

Country differences and substitution limits for 9SiCr

Country comparisons below deliberately distinguish actual source windows from unsupported trade-name substitutions. A comparison entry is not an automatic equivalent. [S1 Annex B; S4; S5]

Country / system Designation and verified difference Substitution limit
China 9SiCr, GB/T 1299-2000; cast C 0.85–0.95 %, delivery 197–241 HBW 10/3000 Current GB/T 1299-2025 requires separate full-table verification
Japan JIS G4401:2009 SK105 carbon-tool contrast: C 1.00–1.10 and Si 0.10–0.35 %, versus GB C 0.85–0.95 and Si 1.20–1.60 %. No corresponding JIS alloy grade established here; JIS decarburization HV is not this hardening-test HRC
United States A681-08 O1 is a contrast, not an assigned counterpart: C 0.85–1.00 and Cr 0.40–0.70 %, versus this GB C 0.85–0.95 and Cr 0.95–1.25 %. Similar tooling use does not eliminate alloy or acceptance differences. Informative association or selected window overlap is not identical chemistry, form, delivery condition or specimen acceptance
Germany / ISO-based procurement No exact DIN/EN/ISO counterpart established by the cited GB table; specify the actual national adoption and edition Do not inherit an ISO steel number or a later national chemistry window from a commercial cross-reference

Why choose SHH STEEL for 9SiCr

SHH STEEL produces and exports 9SiCr tooling stock with an explicit edition and product-form agreement. We distinguish cast chemistry, delivery hardness and reference specimen response rather than advertising a universal final-tool hardness.

  • Review the actual plate or flat manufacturing and acceptance basis.
  • Maintain heat identification and agreed inspection reporting.
  • Review substitutions against complete source editions.
  • Agree any optional condition or supplementary testing before confirmation.

Inspection and enquiry planning for 9SiCr

Enquiry item Required detail
Grade and standard 9SiCr; state the governing edition rather than only GB/T 1299
Product form Flat bar or independently specified plate; manufacturing route and finish
Dimensions Thickness × width × length, quantity and machining allowance
Condition and hardness Annealed; 197–241 HBW 10/3000 on the historical basis, or expressly agreed different requirement
Test verification Cast/product analysis, delivery hardness, specimen-test guarantee/report requirement and sampling basis
Inspection Certificate type, heat traceability, surface/decarburization and any additional agreed quality checks
Final tooling / logistics Duty, final-tool acceptance, treatment responsibility, packing, destination and timing

Requested sizes and processes are reviewed for feasibility; this draft is not an unconditional stock or production-performance commitment.

Request a quotation

Request a quotation for GB/T 1299 9SiCr tooling plate or flat stock by email. State the governing edition, actual product form and manufacturing route, quantity, dimensions, drawing, finish and machining allowance. For ordinary rolled plate, identify the separate applicable plate acceptance basis rather than relying only on the historical bar specification.

Confirm the supplied condition and hardness acceptance: this historical annealed row gives 197–241 HBW 10/3000. Specify cast versus product analysis, inspection-document type, traceability, sampling and whether a hardening-test report or an agreed supplier conformity guarantee is required. The source minimum 62 HRC is a specimen-response requirement, not your final tooling specification.

Include surface and decarburization acceptance, flatness and dimensional tolerances, critical edge preparation, cutting requirements and any supplementary NDT or microstructure checks with agreed methods and criteria. Describe tool duty, final properties and production-treatment responsibility separately. For a proposed substitute, attach its complete governing specification and drawing for review. Provide packing, delivery destination and target timing; feasibility and any optional condition are confirmed before acceptance.

Email only: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X