EN 10248-1 S270GP U-Type and Z-Type Steel Sheet Pile
What is EN 10248-1 S270GP U-Type and Z-Type Steel Sheet Pile?
EN 10248-1 S270GP is a hot-rolled steel sheet pile grade in the GP family. S marks a structural steel, 270 is the minimum yield in MPa, and GP is the sheet-pile quality of that standard. This page covers both U-type and Z-type sections in this grade. It is not a geometry-only companion to the live S355GP U-type and Z-type page, and it is not a cold-formed EN 10249 pile.
The chemistry and mechanical figures follow EN 10248-1:2023. The edition named on the order governs acceptance. Not every published section is rolled in every grade; availability has to be confirmed on the enquiry.
Material, Dimensions and the EN 10248-1 S270GP Grade
EN 10248-1 is the material standard. Shape tolerances follow EN 10248-2 as named on the order (the 2024 edition is the current dimensional document on this site’s S355GP page). The 2023 material edition adds a carbon-equivalent cap and a Charpy requirement that were not part of the older 1995 GP tables. Do not mix 1995 chemistry (for example older, looser phosphorus and sulphur caps) into a 2023 certificate.
EN 10248-1 S270GP Sizes: Typical Hot-Rolled U-Type and Z-Type Series
The tables below reuse the typical published hot-rolled U-type and Z-type series already tabulated on the S355GP page. They describe geometry only (type, width, height and thickness). Trade names are not used. These are typographical mill-series references, not an EN 10248-2 size table and not a mill stock list, and not every section is assumed to be available in S270GP.
Swipe horizontally to view all dimensions.
Typical hot-rolled Z-type series, 770 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
Typical hot-rolled Z-type series, 750 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
Typical hot-rolled Z-type series, 700 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
Typical hot-rolled Z-type series, 630 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
Typical hot-rolled U-type mill series
Typical hot-rolled U-type series, 750 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. Duplicate geometries that appear in more than one mill series are listed once. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
Typical hot-rolled U-type series, 600 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. Duplicate geometries that appear in more than one mill series are listed once. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
Typical hot-rolled U-type series, 400 mm effective width. Geometry is given as type × effective width × height × flange thickness, with a second thickness where the web differs from the flange. Duplicate geometries that appear in more than one mill series are listed once. These are published mill-series dimensions, not an EN 10248-2 size table, and trade names are not used.
Swipe horizontally to view all dimensions.
EN 10248-1:2023 S270GP Chemical Composition (Product Analysis)
Product-analysis limits for S270GP are carbon 0.20 % maximum, manganese 1.60 % maximum, phosphorus 0.050 % maximum, sulphur 0.050 % maximum, nitrogen 0.014 % maximum, copper 0.60 % maximum and CEV 0.43 % maximum. Silicon is not specified. These figures are product analysis, not a heat-analysis table. Do not copy the tighter S355GP carbon, manganese, phosphorus, sulphur or CEV caps onto an S270GP order, or the other way around.
Swipe horizontally to view all dimensions.
EN 10248-1:2023 S270GP Mechanical Properties
Minimum yield is 270 MPa, minimum tensile strength is 410 MPa, and minimum elongation is 24 % on L0 = 5.65 sqrt(S0). The 2023 edition requires a minimum KV2 impact energy of 27 J at +20 C. S355GP, on the sister page, uses 355 / 480 / 22 % and 27 J at 0 C; those figures must not be pasted here.
Swipe horizontally to view all dimensions.
Applications and Service Limits for EN 10248-1 S270GP Sheet Piles
S270GP piles are used in cofferdams, retaining walls and general earth-retaining work where this yield class is named. The grade is not a cold-formed EN 10249 quality and not a weathering or marine alloy grade. If the project needs 355 MPa or 430 MPa, or a 0 C impact test, that grade has to be ordered as such.
Near-Equivalents for EN 10248-1 S270GP: Not Automatic Substitutes
S240GP is a lower-yield GP grade; S320GP and S355GP are higher-yield grades with tighter phosphorus, sulphur and CEV limits and, from S355GP upward, a 0 C impact test. JIS A 5528 SY295 is a Japanese U-type sheet-pile grade, not a restamp of S270GP. ASTM A572 Grade 50 sheet piling follows a different standard.
Sourcing EN 10248-1 S270GP U-Type and Z-Type Steel Sheet Piles from SHH STEEL
Send the section type (U or Z), the width, height and thickness, the length, and the EN 10248-1 edition, and name S270GP explicitly. Do not use the S355GP term for this page, and do not create a Z-only duplicate page. SHH STEEL reviews the grade, the section and the certificate before quoting. The size tables are typographical references, not a warehouse list.
EN 10248-1 S270GP FAQs
-
Is this a Z-only duplicate of the S355GP page?
- No. It is a different grade. U-type and Z-type geometry are both tabulated here, using the same typographical series as the S355GP page, which already covers both types for that grade.
-
Does S270GP require a Charpy test?
- Yes, in the 2023 edition: 27 J at +20 C. S355GP and higher use 27 J at 0 C. Do not mix those temperatures.
-
Is every tabulated section available in S270GP?
- Not necessarily. The tables are typographical mill-series references, not a stock list and not a claim that every section is rolled in every grade.
-
Are these product-analysis or heat-analysis limits?
- Product analysis, as given in EN 10248-1:2023. The ordered edition governs.
Conclusion
EN 10248-1:2023 S270GP is the 270 MPa hot-rolled sheet-pile grade, with 410 MPa tensile, 24 % elongation and 27 J at +20 C, tabulated here in both U-type and Z-type typical series. It is not a geometry-only duplicate of the S355GP page. Confirm the grade, the section and the edition on the order.