EN 10025-3 S355N Steel Plate | S355N Fine Grain Structural Steel - SHH STEEL

EN 10025-3 S355N Steel Plate | S355N Fine Grain Structural Steel

EN 10025-3 S355N is a normalized fine-grain structural steel plate with a minimum yield strength of 355 MPa and impact tested at –20°C. It offers high strength, excellent weldability and good toughness for structural applications. SHH STEEL is a China Mill-Direct Exporter supplying S355N steel plate worldwide.
Equivalent material:
ASTM A572 Gr 50 / JIS SM490YA / GB Q355D / ISO E355N
Material Specification:
EN 10025-3 — Delivery: Normalized (N) or Normalized Rolled
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Tolerances
Weldability
Equivalent Material Grades
Applications
Why Choose SHH STEEL
FAQ
Conclusion

What is EN 10025-3 S355N Steel Plate?

As a professional steel plate supplier and China Mill-Direct Exporter, SHH STEEL is pleased to present EN 10025-3 S355N Steel Plate (Material Number: 1.0545).

S355N is a normalized (or normalized rolled) weldable fine-grain structural steel under the European standard EN 10025-3. It provides a minimum yield strength of 355 MPa (for thickness ≤ 16 mm) and is impact tested at –20°C with a minimum energy of 40 J. Compared with the corresponding EN 10025-2 S355 grades, S355N offers a finer grain structure, better toughness and improved weldability. SHH STEEL sources this material directly from leading Chinese steel mills, ensuring competitive mill-direct pricing, stable quality and reliable delivery.

We supply S355N steel plate in thicknesses from 6 mm to 150 mm (thicker plates available on request), widths up to 3000–4000 mm, and lengths up to 12000–18000 mm. Custom cutting, shot blasting and priming services are available. All plates are delivered with full Mill Test Certificates (EN 10204 3.1).

Material Specification

EN 10025-3 S355N steel plate is produced in accordance with EN 10025-3.

Specification Element Requirement SHH STEEL Compliance
Primary Standard EN 10025-3 Full compliance
Steel Grade S355N (1.0545) Confirmed
Delivery Condition Normalized (+N) Confirmed
Product Form Steel Plate Available
Thickness Range 6 mm – 150 mm Custom sizes available
Width / Length Up to 3000–4000 mm / 12000–18000 mm Custom cutting supported
Certification EN 10204 3.1 / 3.2 Available

Chemical Composition

According to EN 10025-3, the chemical composition is specified for both ladle analysis (cast analysis) and product analysis.

Ladle Analysis (Cast Analysis)

Element Max. / Range (%)
Carbon (C) ≤ 0.20
Silicon (Si) ≤ 0.50
Manganese (Mn) 0.90 – 1.65
Phosphorus (P) ≤ 0.030
Sulfur (S) ≤ 0.025
Niobium (Nb) ≤ 0.05
Vanadium (V) ≤ 0.12
Aluminium (Al total) ≥ 0.020
Titanium (Ti) ≤ 0.05
Chromium (Cr) ≤ 0.30
Nickel (Ni) ≤ 0.50
Molybdenum (Mo) ≤ 0.10
Copper (Cu) ≤ 0.55
Nitrogen (N) ≤ 0.015

Product Analysis

Element Max. / Range (%)
Carbon (C) ≤ 0.22
Silicon (Si) ≤ 0.55
Manganese (Mn) 0.85 – 1.75
Phosphorus (P) ≤ 0.035
Sulfur (S) ≤ 0.030
Niobium (Nb) ≤ 0.06
Vanadium (V) ≤ 0.15
Aluminium (Al total) ≥ 0.015
Titanium (Ti) ≤ 0.06
Chromium (Cr) ≤ 0.35
Nickel (Ni) ≤ 0.55
Molybdenum (Mo) ≤ 0.13
Copper (Cu) ≤ 0.60
Nitrogen (N) ≤ 0.017

Note:

  • V + Nb + Ti ≤ 0.22%
  • Mo + Cr ≤ 0.30%
  • The minimum Al content does not apply if sufficient other nitrogen-binding elements are present.

Mechanical Properties

Mechanical properties of EN 10025-3 S355N (longitudinal direction):

Thickness (mm) Yield Strength ReH (min) Tensile Strength Rm Elongation A (min) Impact Energy KV (min)
≤ 16 355 MPa 470 – 630 MPa 22% 40 J at –20°C
> 16 ≤ 40 345 MPa 470 – 630 MPa 22% 40 J at –20°C
> 40 ≤ 63 335 MPa 470 – 630 MPa 22% 40 J at –20°C
> 63 ≤ 80 325 MPa 470 – 630 MPa 21% 40 J at –20°C
> 80 ≤ 100 315 MPa 470 – 630 MPa 21% 40 J at –20°C
> 100 ≤ 150 295 MPa 450 – 600 MPa 21% 40 J at –20°C

Delivery Conditions

SHH STEEL, as a China Mill-Direct Supplier, supplies EN 10025-3 S355N steel plate in the normalized (+N) condition.

Additional options:

  • Shot blasting and shop primer
  • Ultrasonic testing (EN 10160)
  • Z-direction testing (Z15 / Z25 / Z35)
  • Third-party inspection (SGS, BV, TUV, etc.)

Tolerances

Dimensional tolerances for S355N steel plate follow EN 10029 (for plates).

  • Thickness, width and length tolerances according to the ordered class.
  • Flatness according to EN 10029.
  • Edge conditions: Mill edge or cut edge (flame / plasma).

Tighter tolerances can be provided upon request.

Weldability

S355N has excellent weldability due to its fine-grain structure, controlled carbon equivalent and low impurity levels. It can be welded by all conventional methods (SMAW, GMAW, FCAW, SAW).

Recommended welding consumables:

Welding Process Recommended Consumables
SMAW (Stick) E7018, E7016
GMAW (MIG/MAG) ER70S-6
FCAW E71T-1
SAW EM12K + suitable flux

Preheating may be required for thicker plates. Low-hydrogen consumables are recommended for critical applications.

Equivalent Material Grades

Grade Standard Notes
S355N EN 10025-3 —
1.0545 EN Material number
Q355N / Q355D GB/T 1591 Closest Chinese equivalents
A633 Grade C/D (approx.) ASTM Similar fine-grain concept
StE 355 DIN (old) Former designation

Applications

EN 10025-3 S355N is widely used in structural applications requiring high strength and good toughness. Typical uses include:

Application Area Typical Components / Uses (Keywords)
Building Structures Heavy beams, columns, frames – S355N Structural Steel
Bridges Bridge components – S355N Bridge
Machinery Heavy equipment frames – S355N Machinery
Construction High-strength construction – S355N Construction
Offshore & Industrial Structural components – S355N Industrial
General Fabrication Welded fine-grain high-strength structures – S355N Fabrication

Why Choose SHH STEEL

SHH STEEL is a China Mill-Direct Exporter. We maintain long-term strategic cooperation with major Chinese steel mills and act as a first-level (primary) agent. This direct mill supply model allows us to offer competitive mill-direct pricing, faster delivery times, stable and traceable quality, and full Mill Test Certificates (EN 10204 3.1 / 3.2) for EN 10025-3 S355N Steel Plate.

Customers benefit from reliable supply, short lead times and cost-effective solutions for fine-grain structural steel projects worldwide. Our professional export team provides technical support and customized processing services to meet project requirements.

FAQ

What does the “N” in S355N mean?
“N” indicates that the steel is supplied in the normalized condition and meets impact requirements of minimum 40 J at –20°C.
What is the difference between S355N and S355NL?
Both have the same strength level. S355N is impact tested at –20°C (40 J), while S355NL is impact tested at –50°C (27 J), offering better low-temperature toughness.
What is the material number of S355N?
1.0545
Is S355N a fine-grain steel?
Yes. EN 10025-3 grades are normalized fine-grain structural steels with controlled grain size for improved toughness and weldability.

Conclusion

EN 10025-3 S355N (1.0545) Steel Plate from SHH STEEL is a normalized fine-grain structural steel offering high strength, excellent weldability and reliable toughness at –20°C. As a China Mill-Direct Exporter, we provide competitive pricing, fast delivery and consistent quality backed by full mill certifications. Trust SHH STEEL for your S355N fine grain structural steel plate requirements.

Contact SHH STEEL today for stock availability, pricing and technical support. EN 10025-3 S355N Steel Plate, S355N steel plate, S355N fine grain structural steel, EN 10025 S355N, S355N equivalent, S355N supplier, 1.0545

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *