BS 1501 164 Grade 360B Steel Plate | BS 1501 Steel - SHH STEEL

BS 1501 164 Grade 360B Steel Plate

BS 1501-164 Grade 360B is a fully killed, aluminium-treated carbon steel plate for pressure vessels. Heat-analysis carbon is 0.20 % maximum and manganese is 0.40–1.20 %. Yield strength is 255 N/mm² minimum up to 16 mm, and tensile strength is 360–480 N/mm². Suffix B adds characteristic elevated-temperature proof-stress values to those room-temperature tensile properties. Delivery is normalized unless another condition is agreed. SHH STEEL produces and exports 164 Grade 360B plate to the ordered edition, condition and dimensions.
Equivalent Grades:
EN 10028-2 P265GH is a later carbon vessel name (near name only).
Heat Treatment
Normalized, unless an alternative condition is agreed.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is BS 1501-164 Grade 360B plate?

We produce and export BS 1501-164 Grade 360B as fully killed, aluminium-treated carbon steel plate for fired and unfired pressure equipment. Typical service includes welded boilers, vessels and similar parts that specify type 164 grade 360B.

BS 1501-1:1980 lists eight steel types, each with one or more tensile grades and, where Table 1 allows, suffix A or B and optional impact suffixes. This page specifies only 164 Grade 360B. It is not type 151, 154 or 161, grade 400 of type 164, or a BS 1501-2 alloy plate. Suffix B specifies room-temperature tensile properties together with characteristic elevated-temperature values. RT, LT0 and LT20 are impact-test options, not separate grades.

Composition and room-temperature tensile properties on this page follow BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates, the last final edition of Part 1. BS 1501-1:1980 was published on 28 November 1980 and withdrawn on 15 February 1993. It replaced BS 1501: Part 1: 1964 and that edition’s addenda. It was replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Those successor designations are not automatic aliases for the 1980 type-and-grade names. Name the edition or successor standard required on the purchase order.

The chemical and tensile figures below follow BS 1501-1:1980 as tabulated for this designation, including a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 values. BS 1501-2 (alloy plates) and BS 1501-3 (corrosion- and heat-resisting plates, sheet and strip) are different parts of the same historical series.

SHH STEEL produces and exports BS 1501-164 Grade 360B plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for BS 1501-164 Grade 360B

The items below follow BS 1501-1:1980. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates
Official designation BS 1501-164 Grade 360B
Steel type Fully killed aluminium-treated carbon steel
Product form Hot-rolled steel plate (this part does not cover bars, sections, forgings, tubes or stainless sheet)
How designations are listed Type number, tensile grade and suffix A or B; optional LT or RT impact suffixes where Table 1 allows; optional L after types 223, 224 and 225 when nickel is limited to 0.30 %
Applicable thickness Up to and including 150 mm
Usual heat treatment Normalized, unless an alternative condition is agreed.
Chemical analysis Ladle analysis as tabulated for this type and grade in BS 1501-1:1980
Tensile properties Yield strength, tensile strength and elongation, by thickness, from that edition
Our supply We produce and export 164 Grade 360B plate to the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of BS 1501-164 Grade 360B

The figures below are ladle analysis for BS 1501-164 Grade 360B from BS 1501-1:1980. Values are in weight percent and follow BS 1501-1:1980, including a reprint incorporating Amendments No. 1 to No. 3. They are not current EN 10028 values.

Element 164 Grade 360B ladle analysis, BS 1501-1:1980 (wt. %)
Carbon (C) 0.20 max
Silicon (Si) 0.10–0.35
Manganese (Mn) 0.40–1.20
Phosphorus (P) 0.030 max
Sulfur (S) 0.030 max
Aluminium (Al), metallic 0.015 min
Chromium (Cr) 0.25 max
Copper (Cu) 0.30 max
Molybdenum (Mo) 0.10 max
Nickel (Ni) 0.30 max

Figures are ladle analysis as tabulated for type 164 grade 360 in BS 1501-1:1980. For plates over 63 mm thick the maximum carbon content is 0.22 %. Determination of total aluminium is deemed to meet the metallic aluminium requirement if the value obtained is not less than 0.018 %. The combined total of residual chromium, copper, molybdenum and nickel is 0.70 % maximum. Nitrogen shall not exceed 0.012 %. To reduce the risk of hot shortness, copper (%) plus ten times tin (%) shall not exceed 0.4 %. The 1980 edition allows the purchaser to specify tighter phosphorus and sulfur limits. Elevated-temperature numerical values for suffix B belong in Appendix E and should be taken from the edition named on the order.

Tensile and related properties for BS 1501-164 Grade 360B

164 Grade 360B has thickness-dependent yield strength, tensile strength and elongation. Values below are from BS 1501-1:1980, including a reprint incorporating Amendments No. 1 to No. 3, and are not current EN 10028 values. Strength values are in N/mm², equivalent to MPa.

Thickness Tensile strength Rm, N/mm² Yield strength Re, N/mm² min Elongation A, % min
Over 3 mm up to and including 16 mm 360–480 255 25
Over 16 mm up to and including 40 mm 360–480 235 25
Over 40 mm up to and including 63 mm 360–480 220 24
Over 63 mm up to and including 100 mm 360–480 Reduced by the 1 % per 5 mm rule 23
Over 100 mm up to and including 150 mm 360–480 Reduced by the 1 % per 5 mm rule 23

The tensile window is that stated for this type 164 grade in BS 1501-1:1980. Type 164 covers plates up to and including 150 mm. For plates over 63 mm up to and including 150 mm, yield strength is the 40 mm to 63 mm value reduced by 1 % for each 5 mm or part thereof increase in thickness. If specified, Charpy V-notch values for plates up to and including 63 mm shall comply with the table below (RT, LT0 or LT20). Impact values for plates over 63 mm shall be agreed at enquiry. Those impact suffixes are ordering options, not separate product pages.

Minimum average Charpy V-notch energy for type 164 plates up to and including 63 mm thick, when an impact suffix is specified, from BS 1501-1:1980. Values for plates over 63 mm shall be agreed at enquiry.

Test temperature Minimum average of three, J
Room temperature (RT) 41
0 °C (LT0) 31
−20 °C (LT20) 27

Suffix B specifies characteristic elevated-temperature yield or 0.2 % proof-stress values in Appendix E. Those high-temperature figures should be taken from the edition named on the order.

Delivery conditions for BS 1501-164 Grade 360B

Type 164 is supplied as fully killed, aluminium-treated carbon steel plate. The 1980 text specifies supply in the normalized condition, unless an alternative condition of supply is agreed between the purchaser and the manufacturer. Name the required delivery condition on the purchase order.

If the project has moved to EN 10028-2 or EN 10028-3, order the successor designation and edition expressly. A later name is not by itself a substitute instruction.

The purchase order should name the official designation including the A or B suffix, any required impact suffix, thickness, width and length, the delivery condition, any extra tests, and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

BS 1501-1:1980 does not set a welding procedure. Type 164 is a fully killed, aluminium-treated carbon vessel plate intended for welded pressure equipment. Welding and thermal cutting should be qualified for the carbon content, thickness and delivery condition.

Heat input and any required post-weld heat treatment belong in the project specification.

Form, appearance, dimensions and thickness tolerances

Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate tolerances when that standard is specified.

Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.

Applications and specification limits

We produce and export 164 Grade 360B plate as fully killed, aluminium-treated carbon steel plate for fired and unfired pressure equipment. Typical service includes welded boilers, vessels and similar parts that specify type 164 grade 360B. The 1980 type 164 clauses cover plates up to and including 150 mm thick in grades 360 and 400. This page specifies grade 360 only.

BS 1501-1:1980 is a historical carbon and carbon-manganese plate standard for pressure purposes. It is not the current EN 10028-2 or EN 10028-3 order unless that successor standard is written on the enquiry, and it is not a BS 1501-2 alloy, BS 1501-3 stainless, BS 1502 bar or BS 1503 forging order.

Compare BS 1501-164 Grade 360B with other steel plates

164 Grade 360B is a BS 1501-1:1980 pressure-vessel plate. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
BS 1501-164 Grade 360B (this plate) BS 1501-1:1980 official designation Normalized, unless an alternative condition is agreed. Yield 255 N/mm² minimum up to 16 mm; tensile 360–480 N/mm², with suffix B elevated-temperature properties Typical service includes welded boilers and vessels that specify type 164 grade 360B A different standard, later EN name, or 1980 type is not an automatic substitute
EN 10028-2 P265GH Non-alloy elevated-temperature vessel plate, steel number 1.0425 As specified in EN 10028-2 Published yield 265 MPa and tensile 410–530 MPa Modern European carbon boiler and vessel plate Related carbon class only; a later EN name is not an automatic substitute
GB/T 713 Q245R Later Chinese carbon vessel plate As specified in GB/T 713 Published yield 245 MPa and tensile 400–520 MPa Modern Chinese carbon boiler and vessel plate Related carbon class only
ASTM A516 Grade 60 ASTM carbon vessel plate As specified in ASTM A516/A516M Published yield 220 MPa and tensile 415–550 MPa Carbon pressure-vessel plate to the ASTM book Related product form only

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. A later EN 10028 designation does not by itself authorize substitution. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United Kingdom (historical) BS 1501-1:1980 164 Grade 360A Same type and tensile grade with the opposite A/B suffix Not an automatic substitute; suffix B adds characteristic elevated-temperature values
United Kingdom (historical) BS 1501-1:1980 161 Grade 360B Same tensile grade as a fully killed type 161 plate without a specified metallic-aluminium minimum. Type 164 has a higher room-temperature yield (255 N/mm² versus 205 N/mm² up to 16 mm for grade 360, or 275 N/mm² versus 225 N/mm² for grade 400) and optional RT, LT0 and LT20 impact tests. A different 1980 type, not an automatic substitute
Europe EN 10028-2 P265GH (1.0425) Later non-alloy elevated-temperature vessel plate. Live published yield 265 MPa and tensile 410–530 MPa, against 255 N/mm² and 360–480 N/mm² for 164 Grade 360. Near name only
United States ASTM A516/A516M Grade 60 Carbon vessel plate. Live published yield 220 MPa and tensile 415–550 MPa. Related product form only
China GB/T 713 Q245R Later Chinese carbon vessel plate. Live published yield 245 MPa and tensile 400–520 MPa. Related carbon class only

Why choose SHH STEEL for BS 1501-164 Grade 360B

  • We produce and export BS 1501-164 Grade 360B pressure-vessel steel plate
  • We review the enquiry for edition, designation, delivery condition, dimensions and extra tests
  • We keep the 1980 type, tensile grade and A/B suffix distinct from later EN 10028 names and from BS 1501-2 / BS 1501-3
  • We match documentation to what the purchase order requires

How to enquire for BS 1501-164 Grade 360B plate

Item What to specify
Standard and designation BS 1501-164 Grade 360B and the edition required
Or successor standard EN 10028-2 or EN 10028-3 designation and edition, if that is what the project now requires
Delivery condition Normalized, unless an alternative condition is agreed.
Dimensions Required thickness, width and length
Chemistry Ladle analysis to BS 1501-1:1980, or to another named edition
Mechanical tests Yield strength, tensile strength, elongation and, where specified, elevated-temperature or impact tests to the named edition
Other tests Ultrasonic examination or other extra tests only when written on the order
Documentation State the inspection document type required by the project

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Is BS 1501 still a current product standard?
No. BS 1501-1:1980 is the last final edition of Part 1. It was withdrawn on 15 February 1993 and replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Projects still using the 1980 designation should name that edition on the order.
Which edition do the tables on this page follow?
They follow BS 1501-1:1980, including tabulated values from a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 tables. Specify the edition or successor standard required on the purchase order.
Does BS 1501-1 cover alloy or stainless pressure-vessel plates?
No. Part 1 covers carbon and carbon-manganese plates. Alloy plates belong to BS 1501-2:1988. Corrosion- and heat-resisting plates, sheet and strip belong to BS 1501-3:1990. Bars and sections belong to BS 1502, and forgings to BS 1503. This page is 164 Grade 360B only.
Can P265GH be used instead of 164 Grade 360B?
Only after a project review. Live P265GH is stated as 265 MPa yield and 410–530 MPa tensile, against 255 N/mm² and 360–480 N/mm² for 164 Grade 360. Suffix B elevated values remain those of BS 1501-1:1980 Appendix E. A later EN name is not an automatic substitute.
What should a quotation enquiry include?
BS 1501-164 Grade 360B, the edition required or the successor designation, the delivery condition, plate thickness by width by length, quantity, any extra tests, and the inspection document required.

Request a quotation

Contact SHH STEEL for a quotation for BS 1501-164 Grade 360B steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the edition (BS 1501-1:1980 or a named successor such as EN 10028-2 or EN 10028-3), the A or B suffix, any required impact suffix, the delivery condition and any specimen heat treatment. If your project requires ultrasonic examination, a stated impact temperature or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X