BS 1501 151 Grade 400B Steel Plate | BS 1501 Steel - SHH STEEL

BS 1501 151 Grade 400B Steel Plate

BS 1501-151 Grade 400B is a semi-killed or fully killed carbon steel plate for pressure vessels. Heat-analysis carbon is 0.20 % maximum and manganese is 0.50–1.30 %. Yield strength is 225 N/mm² minimum up to 16 mm, and tensile strength is 400–520 N/mm². Suffix B adds characteristic elevated-temperature proof-stress values to those room-temperature tensile properties. Delivery may be normalized, or hot finished through 40 mm if properties are met. SHH STEEL produces and exports 151 Grade 400B plate to the ordered edition, condition and dimensions.
Equivalent Grades:
EN 10028-2 P265GH is a later carbon vessel name (near name only).
Heat Treatment
Normalized; hot-finished permitted through 40 mm.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is BS 1501-151 Grade 400B plate?

We produce and export BS 1501-151 Grade 400B as semi-killed or fully killed carbon steel plate for fired and unfired pressure equipment. Typical service includes welded boilers, vessels and similar parts that specify type 151 grade 400B.

BS 1501-1:1980 lists eight steel types, each with one or more tensile grades and, where Table 1 allows, suffix A or B and optional impact suffixes. This page specifies only 151 Grade 400B. It is not type 154, 161 or 164, grade 360 or 430 of type 151, or a BS 1501-2 alloy plate. Suffix B specifies room-temperature tensile properties together with characteristic elevated-temperature values.

Composition and room-temperature tensile properties on this page follow BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates, the last final edition of Part 1. BS 1501-1:1980 was published on 28 November 1980 and withdrawn on 15 February 1993. It replaced BS 1501: Part 1: 1964 and that edition’s addenda. It was replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Those successor designations are not automatic aliases for the 1980 type-and-grade names. Name the edition or successor standard required on the purchase order.

The chemical and tensile figures below follow BS 1501-1:1980 as tabulated for this designation, including a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 values. BS 1501-2 (alloy plates) and BS 1501-3 (corrosion- and heat-resisting plates, sheet and strip) are different parts of the same historical series.

SHH STEEL produces and exports BS 1501-151 Grade 400B plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for BS 1501-151 Grade 400B

The items below follow BS 1501-1:1980. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates
Official designation BS 1501-151 Grade 400B
Steel type Semi-killed or fully killed carbon steel
Product form Hot-rolled steel plate (this part does not cover bars, sections, forgings, tubes or stainless sheet)
How designations are listed Type number, tensile grade and suffix A or B; optional LT or RT impact suffixes where Table 1 allows; optional L after types 223, 224 and 225 when nickel is limited to 0.30 %
Applicable thickness Up to and including 100 mm
Usual heat treatment Normalized; hot-finished permitted through 40 mm.
Chemical analysis Ladle analysis as tabulated for this type and grade in BS 1501-1:1980
Tensile properties Yield strength, tensile strength and elongation, by thickness, from that edition
Our supply We produce and export 151 Grade 400B plate to the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of BS 1501-151 Grade 400B

The figures below are ladle analysis for BS 1501-151 Grade 400B from BS 1501-1:1980. Values are in weight percent.

Element 151 Grade 400B ladle analysis, BS 1501-1:1980 (wt. %)
Carbon (C) 0.20 max
Silicon (Si) 0.35 max
Manganese (Mn) 0.50–1.30
Phosphorus (P) 0.030 max
Sulfur (S) 0.045 max
Chromium (Cr) 0.25 max
Copper (Cu) 0.30 max
Molybdenum (Mo) 0.10 max
Nickel (Ni) 0.30 max

Figures are ladle analysis as tabulated for this designation in BS 1501-1:1980. Type 151 may be supplied semi-killed or fully killed; when the steel is fully killed, silicon shall comply with table 16 (0.35 % maximum). Aluminium may be used in addition to silicon for deoxidation. The combined total of residual chromium, copper, molybdenum and nickel is 0.70 % maximum. Nitrogen shall not exceed 0.012 %. The 1980 edition allows the purchaser to specify tighter phosphorus and sulfur limits. Elevated-temperature numerical values for suffix B belong in Appendix D and should be taken from the edition named on the order.

Tensile and related properties for BS 1501-151 Grade 400B

151 Grade 400B has thickness-dependent yield strength, tensile strength and elongation. Values below are from BS 1501-1:1980. Strength values are in N/mm², equivalent to MPa.

Thickness Tensile strength Rm, N/mm² Yield strength Re, N/mm² min Elongation A, % min
Over 3 mm up to and including 16 mm 400–520 225 24
Over 16 mm up to and including 40 mm 400–520 215 24
Over 40 mm up to and including 63 mm 400–520 205 23
Over 63 mm up to and including 100 mm 400–520 200 22

The tensile window is that stated for this type 151 grade in BS 1501-1:1980. Type 151 clauses cover plates up to and including 100 mm; there is no 100 mm to 150 mm band in table 17. Impact properties are not listed as an available option for type 151 in the 1980 property-options table.

Suffix B specifies characteristic elevated-temperature yield or 0.2 % proof-stress values in the 1980 appendices. Those high-temperature figures should be taken from the edition named on the order.

Delivery conditions for BS 1501-151 Grade 400B

Type 151 is supplied as semi-killed or fully killed carbon steel plate. The 1980 text specifies supply in the normalized condition, except that the manufacturer may omit normalizing for plates up to and including 40 mm thick provided all specified properties are met in the hot-finished condition. The purchaser may require normalized plate, or normalized test samples, through 40 mm if agreed at enquiry. Name the required delivery condition on the purchase order.

If the project has moved to EN 10028-2 or EN 10028-3, order the successor designation and edition expressly. A later name is not by itself a substitute instruction.

The purchase order should name the official designation including the A or B suffix, any required impact suffix, thickness, width and length, the delivery condition, any extra tests, and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

BS 1501-1:1980 does not set a welding procedure. Type 151 is a carbon vessel plate intended for welded pressure equipment. Welding and thermal cutting should be qualified for the carbon content, thickness and delivery condition.

Heat input and any required post-weld heat treatment belong in the project specification.

Form, appearance, dimensions and thickness tolerances

Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate tolerances when that standard is specified.

Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.

Applications and specification limits

We produce and export 151 Grade 400B plate as semi-killed or fully killed carbon steel plate for fired and unfired pressure equipment. Typical service includes welded boilers, vessels and similar parts that specify type 151 grade 400B. The 1980 type 151 clauses cover plates up to and including 100 mm thick in grades 400, 400 and 430. This page specifies grade 400 only.

BS 1501-1:1980 is a historical carbon and carbon-manganese plate standard for pressure purposes. It is not the current EN 10028-2 or EN 10028-3 order unless that successor standard is written on the enquiry, and it is not a BS 1501-2 alloy, BS 1501-3 stainless, BS 1502 bar or BS 1503 forging order.

Compare BS 1501-151 Grade 400B with other steel plates

151 Grade 400B is a BS 1501-1:1980 pressure-vessel plate. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
BS 1501-151 Grade 400B (this plate) BS 1501-1:1980 official designation Normalized; hot-finished permitted through 40 mm. Yield 225 N/mm² minimum up to 16 mm; tensile 400–520 N/mm², with suffix B elevated-temperature properties Typical service includes welded boilers and vessels that specify type 151 grade 400B A different standard, later EN name, or 1980 type is not an automatic substitute
EN 10028-2 P265GH Non-alloy elevated-temperature vessel plate, steel number 1.0425 As specified in EN 10028-2 Published yield 265 MPa and tensile 410–530 MPa Modern European carbon boiler and vessel plate Related carbon class only; a later EN name is not an automatic substitute
GB/T 713 Q245R Later Chinese carbon vessel plate As specified in GB/T 713 Published yield 245 MPa and tensile 400–520 MPa Modern Chinese carbon boiler and vessel plate Related carbon class only
ASTM A516 Grade 60 ASTM carbon vessel plate As specified in ASTM A516/A516M Published yield 220 MPa and tensile 415–550 MPa Carbon pressure-vessel plate to the ASTM book Related product form only

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. A later EN 10028 designation does not by itself authorize substitution. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United Kingdom (historical) BS 1501-1:1980 151 Grade 400A Same type and tensile grade with the opposite A/B suffix Not an automatic substitute; suffix B adds characteristic elevated-temperature values
United Kingdom (historical) BS 1501-1:1980 161 Grade 400B Same tensile grade as a fully killed type 161 plate. Type 161 has silicon 0.10–0.35 %, sulfur 0.030 % maximum and a 150 mm thickness limit, whereas type 151 allows semi-killed or fully killed steel, silicon 0.35 % maximum, sulfur 0.045 % maximum and a 100 mm thickness limit. A different 1980 type, not an automatic substitute
Europe EN 10028-2 P265GH (1.0425) Later non-alloy elevated-temperature vessel plate. Live published yield 265 MPa and tensile 410–530 MPa, against 225 N/mm² and 400–520 N/mm² for 151 Grade 400. Near name only; a later EN designation is not an automatic substitute
United States ASTM A516/A516M Grade 60 Carbon vessel plate. Live published yield 220 MPa and tensile 415–550 MPa. Related product form only
China GB/T 713 Q245R Later Chinese carbon vessel plate. Live published yield 245 MPa and tensile 400–520 MPa, matching the 151 Grade 400 tensile window. Related carbon class only; yield and deoxidation rules differ

Why choose SHH STEEL for BS 1501-151 Grade 400B

  • We produce and export BS 1501-151 Grade 400B pressure-vessel steel plate
  • We review the enquiry for edition, designation, delivery condition, dimensions and extra tests
  • We keep the 1980 type, tensile grade and A/B suffix distinct from later EN 10028 names and from BS 1501-2 / BS 1501-3
  • We match documentation to what the purchase order requires

How to enquire for BS 1501-151 Grade 400B plate

Item What to specify
Standard and designation BS 1501-151 Grade 400B and the edition required
Or successor standard EN 10028-2 or EN 10028-3 designation and edition, if that is what the project now requires
Delivery condition Normalized; hot-finished permitted through 40 mm.
Dimensions Required thickness, width and length
Chemistry Ladle analysis to BS 1501-1:1980, or to another named edition
Mechanical tests Yield strength, tensile strength, elongation and, where specified, elevated-temperature or impact tests to the named edition
Other tests Ultrasonic examination or other extra tests only when written on the order
Documentation State the inspection document type required by the project

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Is BS 1501 still a current product standard?
No. BS 1501-1:1980 is the last final edition of Part 1. It was withdrawn on 15 February 1993 and replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Projects still using the 1980 designation should name that edition on the order.
Which edition do the tables on this page follow?
They follow BS 1501-1:1980, including tabulated values from a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 tables. Specify the edition or successor standard required on the purchase order.
Does BS 1501-1 cover alloy or stainless pressure-vessel plates?
No. Part 1 covers carbon and carbon-manganese plates. Alloy plates belong to BS 1501-2:1988. Corrosion- and heat-resisting plates, sheet and strip belong to BS 1501-3:1990. Bars and sections belong to BS 1502, and forgings to BS 1503. This page is 151 Grade 400B only.
Can Q245R be used instead of 151 Grade 400B?
Only after a project review. Live Q245R is stated as 245 MPa yield and 400–520 MPa tensile. 151 Grade 400 shares that tensile window but has a yield of 225 N/mm² minimum up to 16 mm and may be semi-killed. Suffix B elevated values remain those of BS 1501-1:1980 Appendix D.
What should a quotation enquiry include?
BS 1501-151 Grade 400B, the edition required or the successor designation, the delivery condition, plate thickness by width by length, quantity, any extra tests, and the inspection document required.

Request a quotation

Contact SHH STEEL for a quotation for BS 1501-151 Grade 400B steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the edition (BS 1501-1:1980 or a named successor such as EN 10028-2 or EN 10028-3), the A or B suffix, any required impact suffix, the delivery condition and any specimen heat treatment. If your project requires ultrasonic examination, a stated impact temperature or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X