What is ASTM A681 P4 plate?
ASTM A681 P4 Tool Steel Plate is a low-carbon chromium-molybdenum mould steel. Carbon is 0.12 % maximum, chromium 4.00–5.25 % and molybdenum 0.40–1.00 %, substantially different from P2. A higher-chromium low-carbon mould route specified by chemistry rather than a hot-work-grade nickname.
Numerical requirements here follow the finalized ASTM A681-08 (2008) text, approved 1 October 2008. This is a dated published-standard reference, not a claim that a later edition has identical tables. Plate, sheet, strip, bars and forgings are expressly within the wrought-product scope.
Chromium overlap with some hot-work steels is not a hot-work equivalence or a finished-mould hardness guarantee.
SHH STEEL produces and exports P4 plate against the agreed grade, condition and inspection basis. See ASTM A681 within Tool and Die Steel Plates.
Material specification for P4
| Parameter | Requirement / scope |
|---|---|
| Standard / identity | ASTM A681-08; P4, UNS T51604; mould steel |
| Product scope | Wrought plate, sheet, strip, bar and other forms within clause 1.2 |
| Manufacture | Electric melting unless otherwise specified; refinement under clause 5.1 |
| Chemistry | Verified Table 1 analysis and applicable footnotes; product-analysis tolerances already included |
| Delivery / hardness | Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified |
| Cold-drawn maximum | No numerical value listed in Table 2 for this type |
| Response-to-hardening | Table 3 note 4 excludes P-type response testing; no type-specific specimen-response HRC row |
| Lot | Shipment by heat, type, size and shape, clause 12.1 |
| Units | Inch-pound values govern; SI conversions informational |
Chemical composition of P4
Table 1 values below are mass percent. Listed limits already include product-analysis tolerances; do not add a separate allowance. An ellipsis means no listed limit for that element here, not a zero-content guarantee.
| Element | A681-08 Table 1 chemical requirement (wt. %) |
|---|---|
| Carbon (C) | 0.12 max |
| Manganese (Mn) | 0.20–0.60 |
| Phosphorus (P) | 0.030 max |
| Sulfur (S) | 0.030 max |
| Silicon (Si) | 0.10–0.40 |
| Chromium (Cr) | 4.00–5.25 |
| Vanadium (V) | Not specified in Table 1 |
| Tungsten (W) | Not specified in Table 1 |
| Molybdenum (Mo) | 0.40–1.00 |
Unless otherwise specified, nickel plus copper shall not exceed 0.75 % (Table 1 note A). Where specified, sulfur may be 0.06–0.15 % to improve machinability (note D); this optional resulfurized route is distinct from the normal 0.030 % sulfur maximum. Heat analysis is required under clause 6.1. Clause 6.2 purchaser analysis is specifically described for finished bars/forgings; it is not a substitute plate sampling method or permission to widen the limits.
Delivery hardness and final mould acceptance for P4
The P4 Table 2 basis is: Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified. A numerical cold-drawn maximum is not supplied by the printed row. It must not be filled from a nearby tool-steel type.
| Acceptance item | Basis |
|---|---|
| Supply condition | Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified |
| Hardening-response specimen | Table 3 note 4 excludes P-type response testing; no type-specific specimen-response HRC row |
| Final mould properties | Agreed against the applicable source and order; not an inherited tool-family HRC |
| Case/core requirements | Specify applicable depth, hardness and inspection if required; no numbers inferred |
Clause 3.1.8.1 identifies P2–P6 as carburizing mould steels: after machining or hubbing they require carburizing to obtain the intended hard surface. The annealed maximum is not final case hardness, core strength or case depth.
Delivery condition and response-test treatment for P4
Specify the actual supplied condition for P4: Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified. The ordered dimensions, finish and final mould requirements remain separate acceptance items.
Table 3 note 4 states that P-types shall not be tested for response to heat treatment. Its explanation identifies P2–P6 as used in the carburized condition and P20 as normally prehardened. P21 likewise has no Table 3 treatment row; its normally prehardened basis is supplied by clause 3.1.8.2 and Table 2 footnote A.
No preheat, austenitizing temperature, holding time, quench medium, tempering or ageing recipe is assigned from an absent response-test row. Use the applicable source and order for any subsequent treatment. A producer typical range is not an ASTM limit unless separately adopted in the order.
Welding, cutting and grinding P4
P4 is an alloy tool steel, not a readily weldable general fabrication plate. Tool repair welding requires a procedure matched to chemistry, prior condition, section, restraint and the intended final heat treatment. No generic preheat or post-weld temperature is prescribed here.
Thermal cutting, electrical discharge machining and grinding can leave altered layers or local cracking at the tool surface. Allow for finishing and inspect critical edges before final service. Grinding burn and tensile surface stresses can defeat an otherwise suitable die chemistry. Chromium overlap with some hot-work steels is not a hot-work equivalence or a finished-mould hardness guarantee.
Plate/flat dimensions, surface quality and inspection
Clause 10.1 invokes the applicable dimensional tables. Hot-rolled sheet/plate has its own Table 24 thickness tolerances and machining allowances, Table 25 trimmed width/length tolerances, Table 26 flatness and Table 27 camber. Flat bar or machined stock must use its applicable form-specific table rather than a round-bar diameter tolerance.
As a Table 24 example, hot-rolled plate over 0.500 through 1.000 in. (12.7–25.4 mm) has a 0.100-in. (2.54-mm) thickness tolerance, all over the specified thickness, and a 0.063-in. (1.60-mm) machining allowance. The table notes relate maximum decarburization to 80 % of the machining allowance per side and permit additional cleanup for flatness. This example is a tolerance reference, not a stock or capacity range.
Under clause 9.2, ground/polished, ground-finished or machine-finished material must be free of scale and decarburization. For other finishes, apply the appropriate size/shape limits and agree any tighter acceptance. Macrostructure is examined under clause 8/ASTM A561 for harmful porosity, segregation, inclusions, pipe and cracks; apply the appropriate composition/size rating, not an invented universal plate class.
Applications and selection limits for P4
Engineering applications considered for P4 include carburized mould cavities and tooling inserts. A higher-chromium low-carbon mould route specified by chemistry rather than a hot-work-grade nickname. The standard classifies composition; the exact finished die, duty cycle and heat treatment still require engineering qualification.
Carbon is 0.12 % maximum, chromium 4.00–5.25 % and molybdenum 0.40–1.00 %, substantially different from P2.
Chromium overlap with some hot-work steels is not a hot-work equivalence or a finished-mould hardness guarantee. Corrosion protection and thermal management are separate design matters; mould steel is not a pressure-vessel or stainless-service specification.
Compare P4 with published tool and engineering plates
The following own pages are already published. These are material-selection contrasts, not substitutes; tool performance cannot be inferred from carbon content or a shared plate form.
| Material | Type / chemistry | Condition | Property basis | Typical route | Substitution limit |
|---|---|---|---|---|---|
| P4 (this plate) | low-carbon chromium-molybdenum mould steel | Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified | P-type response testing excluded; no specimen-response HRC assigned | Mould tooling; condition-specific route | Not a carbon cutting-tool or machinery-alloy substitute |
| JIS G4401 SK140 Tool Steel Plate | Carbon tool steel; published C 1.30–1.50 % | As-hot-rolled unless otherwise specified; annealed/cold-rolled by agreement | JIS G4401:2009 plate/strip hardness basis; not A681 Table 3 | Cutting/file or edge-tool blanks as appropriate | High-carbon cutting-tool route; lacks this specified tool-steel alloy balance |
| JIS G4401 SK120 Tool Steel Plate | Carbon tool steel; published C 1.15–1.25 % | As-hot-rolled unless otherwise specified; annealed/cold-rolled by agreement | JIS G4401:2009 plate/strip hardness basis; not A681 Table 3 | Cutting/file or edge-tool blanks as appropriate | High-carbon cutting-tool route; lacks this specified tool-steel alloy balance |
| ASTM A829 4140 Alloy Steel Plate | Cr-Mo engineering plate; published reference C 0.36–0.44 % | Ordered condition on existing page | Chemistry-ordered plate; no automatic A681 tool-hardness/response package | Machinery parts and later heat-treated components | Structural-quality engineering alloy, not an A681 matching tool-steel specification |
International comparisons and substitution limits for P4
The JIS comparison below uses finalized JIS G 4404:2015 Table 5. Values in each pair are JIS first, ASTM second; all are wt. %. The ISO name, where present, is the JIS informational Annex JA.1 association, not a direct ASTM-certified equivalent.
| Country / system | Designation | Actual differences / form | Condition and substitution limit |
|---|---|---|---|
| United States | ASTM A681-08 P4, UNS T51604 | This wrought tool-steel specification, including plate | Table 2 condition basis; P-type Table 3 response testing excluded |
| Japan | JIS G 4404:2015 SKD61 | JIS SKD61 C 0.35–0.42, Cr 4.80–5.50 and Mo 1.00–1.50 versus P4 C 0.12 maximum, Cr 4.00–5.25 and Mo 0.40–1.00. JIS requires V 0.80–1.15; ASTM P4 has no listed V range. | Hot-work versus low-carbon mould contrast; partial chromium overlap is not equivalence. JIS annealed delivery, plate/flat acceptance and test regimes differ. The cited JIS sulfur limit is not automatically the ASTM limit. |
| International / European ISO route | X40CrMoV5-1 | JIS Annex JA.1 informational comparison only; no complete ISO chemical window is asserted identical | Confirm actual ISO edition, product form, heat-treatment and acceptance requirements; no direct DIN/ASTM alias is inferred |
A681 Table 3 measures minimum response to hardening; JIS G4404 Table 10 and G4403 Table 7 HV values instead define practical-decarburization depth. Those regimes are not interchangeable. Similar principal chemistry does not establish equal manufacturing, cleanliness, carbide distribution or finished-tool performance.
Why choose SHH STEEL for P4
SHH STEEL produces and exports P4 plate against the specified chemistry, delivery condition and inspection plan. We distinguish the supplied mould-stock condition from separately agreed final case/core or treated properties.
- Identify the correct ASTM edition and chemical footnotes.
- Keep plate dimensions, finish and machining allowance explicit.
- Agree hardness acceptance without inventing an excluded specimen test.
- Maintain heat traceability and inspection documentation.
Enquiry and inspection planning for P4
| Enquiry item | What to specify |
|---|---|
| Type / edition | P4, ASTM edition and any additional drawing specification |
| Dimensions | Plate/flat, thickness × width × length, quantity, finish and machining allowance |
| Supply / acceptance | Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified |
| Final mould basis | Intended duty and applicable source for final properties or subsequent treatment |
| Inspection | Heat analysis, agreed supply hardness, dimensions, surface/decarburization and additional NDT if specified |
| Reporting / delivery | Required reports, heat identification, destination, packing and target timing |
No numerical finished-mould property, stock size or process capability is guaranteed without enquiry review.
FAQ
-
What distinguishes P4?
- Carbon is 0.12 % maximum, chromium 4.00–5.25 % and molybdenum 0.40–1.00 %, substantially different from P2. Chromium overlap with some hot-work steels is not a hot-work equivalence or a finished-mould hardness guarantee.
-
What supplied hardness does the reference specify?
- Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified. This is not a final-mould performance guarantee.
-
What is the minimum Table 3 response HRC?
- P-type response testing is excluded by Table 3 note 4; no type-specific test cycle or minimum HRC is assigned here. Use the type-specific condition and agreed final acceptance rather than importing another tool family test.
-
Does the reference include mould plate or only bars?
- Clause 1.2 includes wrought plate. Use the applicable plate/flat dimensional and finish rules; do not transfer bar tolerances or another type specimen requirement to the plate.
-
Is the foreign comparison a direct substitute?
- Hot-work versus low-carbon mould contrast; partial chromium overlap is not equivalence. JIS SKD61 C 0.35–0.42, Cr 4.80–5.50 and Mo 1.00–1.50 versus P4 C 0.12 maximum, Cr 4.00–5.25 and Mo 0.40–1.00. JIS requires V 0.80–1.15; ASTM P4 has no listed V range. Compare chemistry, product form, delivery condition and final acceptance before substitution.
Request a quotation
Request a quotation for ASTM A681 P4 mould steel plate or flat stock. Send the required edition, dimensions, quantity, finish and machining allowance, together with the drawing and intended mould duty. Identify the supplied condition explicitly: Annealed: 131 BHN maximum, Table 2; final carburized condition separately specified.
Specify the governing hardness acceptance and reporting basis rather than copying a generic tool-steel HRC range. P-type response testing is excluded in the reference; no absent specimen cycle is assumed. For final carburized or otherwise treated mould requirements, identify the applicable source and agree case/core properties, treatment responsibility and inspection stages separately.
Include the full chemical requirements and any supplementary quality criteria, heat-traceability needs, surface or decarburization acceptance and any NDT method with its acceptance criteria. For a proposed foreign substitute, provide the complete governing specification and drawing for review of chemistry, form and condition differences.
State whether dimensions are raw blanks or finished sizes; include cutting details, inspection reports, destination, packing and target timing. Any requested process or dimension is reviewed for feasibility before confirmation.