ASTM A681 L2 Tool Steel Plate
What is ASTM A681 L2 plate?
ASTM A681 L2 Tool Steel Plate is a low-alloy special-purpose tool steel. Table 1 allows carbon 0.45–1.00 %, but the Table 3 minimum response applies only to the 0.45–0.55 % carbon type under footnote A. A carbon-selected special-purpose route: lower-carbon structural use and higher-carbon short-run tooling are different requirements.
Numerical requirements here follow the finalized ASTM A681-08 (2008) text, approved 1 October 2008. This is a dated published-standard reference, not a claim that a later edition has identical tables. Plate, sheet, strip, bars and forgings are expressly within the wrought-product scope.
Do not extend the low-carbon specimen response to the full chemistry window. Agree the selected carbon basis and applicable hardness/treatment acceptance before ordering.
SHH STEEL produces and exports L2 plate against the agreed grade, condition and inspection basis. See ASTM A681 within Tool and Die Steel Plates.
Material specification for L2
| Parameter | Requirement / scope |
|---|---|
| Standard / type | ASTM A681-08; L2, UNS T61202; special-purpose low-alloy tool steel |
| Product scope | Available wrought products including hot/cold finished bar, plate, sheet, strip, rod, wire and forgings |
| Manufacture | Electric melting unless otherwise specified; ingot/slab reduction sufficient to refine solidification structure, clause 5.1 |
| Condition | State annealed, hardened and tempered, or other specified condition under ordering clause 4.1.6 |
| Chemistry | Table 1 heat analysis; listed limits already include product-analysis tolerances |
| Annealed hardness | Table 2: 197 BHN maximum |
| Cold-drawn hardness | Table 2: 241 BHN maximum for that condition; not an annealed plate limit |
| Hardening response | Table 3: minimum 53 HRC (0.45–0.55 % carbon type only; Table 3 footnote A) on the prescribed test specimen and treatment |
| Lot | Each shipment of a heat by type, size and shape is a lot, clause 12.1 |
| Unit basis | Inch-pound values govern; parenthetical SI values are informational conversions, clause 1.3 |
Chemical composition of L2
Table 1 values below are mass percent. Listed limits already include product-analysis tolerances; do not add a separate allowance. An ellipsis means no listed limit for that element here, not a zero-content guarantee.
| Element | A681-08 Table 1 chemical requirement (wt. %) |
|---|---|
| Carbon (C) | 0.45–1.00 |
| Manganese (Mn) | 0.10–0.90 |
| Phosphorus (P) | 0.030 max |
| Sulfur (S) | 0.030 max |
| Silicon (Si) | 0.10–0.50 |
| Chromium (Cr) | 0.70–1.20 |
| Vanadium (V) | 0.10–0.30 |
| Tungsten (W) | Not specified in Table 1 |
| Molybdenum (Mo) | 0.25 max |
Unless otherwise specified, nickel plus copper shall not exceed 0.75 % (Table 1 note A). Where specified, sulfur may be 0.06–0.15 % to improve machinability (note D); this optional resulfurized route is distinct from the normal 0.030 % sulfur maximum. Heat analysis is required under clause 6.1. Clause 6.2 purchaser analysis is specifically described for finished bars/forgings; it is not a substitute plate sampling method or permission to widen the limits.
Hardness and minimum hardening response for L2
Table 2 gives L2 maximum annealed hardness of 197 BHN and a separate cold-drawn maximum of 241 BHN. Clause 7.1 refers to ASTM A370 and equivalent Rockwell values. The condition matters: a cold-drawn-flat limit is not automatically the limit for annealed plate.
| Property / regime | Value | Meaning |
|---|---|---|
| Annealed acceptance | 197 BHN max | Specified annealed condition, Table 2 |
| Cold-drawn acceptance | 241 BHN max | Only that delivery condition, Table 2 |
| Minimum response to hardening | 53 HRC (0.45–0.55 % carbon type only; Table 3 footnote A) | Table 3 specimen response after stipulated treatment, not an as-delivered annealed hardness |
| Production tool properties | Defined by the tool specification | A test response does not guarantee arbitrary plate-section or finished-die properties |
Clause 7.2 uses 1/4-in. (6.4-mm) thick disks representing the full cross section or the position midway between center and outer surface. Where form/size is unsuitable, longitudinal specimens may be used; these are at least 3 in. (76 mm) long with parallel flats ground on the original mill surfaces. Clause 7.2.1 uses the average of at least five hardness readings in the stated location, with light-load tests agreed where needed for thin pieces.
Table 3 footnote A restricts the 53 HRC minimum to the 0.45–0.55 % carbon type. Table 1 has a broader 0.45–1.00 % carbon window. No response minimum is inferred here for other L2 carbon selections; agree the applicable source and order acceptance.
Delivery condition and response-test treatment for L2
Specify the delivery condition. An enquiry for annealed machining stock is different from one for hardened-and-tempered material. Table 2 calls the condition annealed; this edition does not impose a blanket spheroidizing temperature or a universal spheroidized-carbide rating. Specify any additional carbide-morphology requirement separately.
| A681-08 Table 3 response-test item | Reference |
|---|---|
| Preheat | 1200 °F (649 °C) |
| Salt-bath austenitizing | 1575 °F (857 °C) |
| Controlled-atmosphere austenitizing | 1600 °F (871 °C) |
| Listed austenitizing time | 5–15 min; apply Table 3 note 2 for furnace/salt method |
| Quench medium | Oil |
| Temper | 400 °F (204 °C); single temper, 2 h |
| Minimum test response | 53 HRC (0.45–0.55 % carbon type only; Table 3 footnote A) |
Table 3 note 1 restricts these austenitizing temperatures to the response-to-hardening test; other combinations may be used for particular applications. Note 2 permits preheat ±25 °F (14 °C), but austenitizing/tempering ±10 °F (5.6 °C). Controlled-atmosphere specimens are held 5–15 min after reaching temperature; salt treatment follows the minimum time indicated. These are test-piece parameters, not a guaranteed production cycle for every plate thickness.
The listed L2 Table 3 response regime and its minimum are for the 0.45–0.55 % carbon type under footnote A. They are not automatically a response requirement for every permitted L2 chemistry.
Welding, cutting and grinding L2
L2 is an alloy tool steel, not a readily weldable general fabrication plate. Tool repair welding requires a procedure matched to chemistry, prior condition, section, restraint and the intended final heat treatment. No generic preheat or post-weld temperature is prescribed here.
Thermal cutting, electrical discharge machining and grinding can leave altered layers or local cracking at the tool surface. Allow for finishing and inspect critical edges before final service. Grinding burn and tensile surface stresses can defeat an otherwise suitable die chemistry. Do not extend the low-carbon specimen response to the full chemistry window. Agree the selected carbon basis and applicable hardness/treatment acceptance before ordering.
Plate/flat dimensions, surface quality and inspection
Clause 10.1 invokes the applicable dimensional tables. Hot-rolled sheet/plate has its own Table 24 thickness tolerances and machining allowances, Table 25 trimmed width/length tolerances, Table 26 flatness and Table 27 camber. Flat bar or machined stock must use its applicable form-specific table rather than a round-bar diameter tolerance.
As a Table 24 example, hot-rolled plate over 0.500 through 1.000 in. (12.7–25.4 mm) has a 0.100-in. (2.54-mm) thickness tolerance, all over the specified thickness, and a 0.063-in. (1.60-mm) machining allowance. The table notes relate maximum decarburization to 80 % of the machining allowance per side and permit additional cleanup for flatness. This example is a tolerance reference, not a stock or capacity range.
Under clause 9.2, ground/polished, ground-finished or machine-finished material must be free of scale and decarburization. For other finishes, apply the appropriate size/shape limits and agree any tighter acceptance. Macrostructure is examined under clause 8/ASTM A561 for harmful porosity, segregation, inclusions, pipe and cracks; apply the appropriate composition/size rating, not an invented universal plate class.
Applications and selection limits for L2
Engineering applications considered for L2 include carbon-selected structural parts and short-run tooling blanks. A carbon-selected special-purpose route: lower-carbon structural use and higher-carbon short-run tooling are different requirements. The standard classifies composition; the exact finished die, duty cycle and heat treatment still require engineering qualification.
Table 1 allows carbon 0.45–1.00 %, but the Table 3 minimum response applies only to the 0.45–0.55 % carbon type under footnote A.
Do not extend the low-carbon specimen response to the full chemistry window. Agree the selected carbon basis and applicable hardness/treatment acceptance before ordering. Corrosion protection and thermal management are separate design matters; cold-work tool steel is not a pressure-vessel or stainless-service specification.
Compare L2 with published tool and engineering plates
The following own pages are already published. These are material-selection contrasts, not substitutes; tool performance cannot be inferred from carbon content or a shared plate form.
| Material | Type / chemistry | Condition | Property basis | Typical route | Substitution limit |
|---|---|---|---|---|---|
| L2 (this plate) | low-alloy special-purpose tool steel | Annealed 197 BHN max; other condition specified | Minimum response 53 HRC (0.45–0.55 % carbon type only; Table 3 footnote A) on Table 3 specimen | Carbon-selected structural parts / short-run tools | Not a carbon cutting-tool or machinery-alloy substitute |
| JIS G4401 SK140 Tool Steel Plate | Carbon tool steel; published C 1.30–1.50 % | As-hot-rolled unless otherwise specified; annealed/cold-rolled by agreement | JIS G4401:2009 plate/strip hardness basis; not A681 Table 3 | Cutting/file or edge-tool blanks as appropriate | High-carbon cutting-tool route; lacks this specified tool-steel alloy balance |
| JIS G4401 SK120 Tool Steel Plate | Carbon tool steel; published C 1.15–1.25 % | As-hot-rolled unless otherwise specified; annealed/cold-rolled by agreement | JIS G4401:2009 plate/strip hardness basis; not A681 Table 3 | Cutting/file or edge-tool blanks as appropriate | High-carbon cutting-tool route; lacks this specified tool-steel alloy balance |
| ASTM A829 4140 Alloy Steel Plate | Cr-Mo engineering plate; published reference C 0.36–0.44 % | Ordered condition on existing page | Chemistry-ordered plate; no automatic A681 tool-hardness/response package | Machinery parts and later heat-treated components | Structural-quality engineering alloy, not an A681 matching tool-steel specification |
International comparisons and substitution limits for L2
The JIS comparison below uses finalized JIS G 4404:2015 Table 3. Values in each pair are JIS first, ASTM second; all are wt. %. The ISO name, where present, is the JIS informational Annex JA.1 association, not a direct ASTM-certified equivalent.
| Country / system | Designation | Actual differences / form | Condition and substitution limit |
|---|---|---|---|
| United States | ASTM A681-08 L2, UNS T61202 | This wrought tool-steel specification, including plate | Table 2 condition maxima; Table 3 response only for 0.45–0.55 % carbon type, footnote A |
| Japan | JIS G 4404:2015 SKS4 | JIS SKS4 C 0.45–0.55 and W 0.50–1.00 versus the full L2 C 0.45–1.00 window and no specified W range. JIS Cr 0.50–1.00 versus L2 0.70–1.20. | Lower-carbon application contrast only. The ASTM response footnote does not make this JIS grade an L2 equivalent. JIS annealed delivery, plate/flat acceptance and test regimes differ. The cited JIS sulfur limit is not automatically the ASTM limit. |
| International / European ISO route | No ISO symbol assigned to the cited JIS grade | JIS Annex JA.1 informational comparison only; no complete ISO chemical window is asserted identical | Confirm actual ISO edition, product form, heat-treatment and acceptance requirements; no direct DIN/ASTM alias is inferred |
A681 Table 3 measures minimum response to hardening; JIS G4404 Table 10 and G4403 Table 7 HV values instead define practical-decarburization depth. Those regimes are not interchangeable. Similar principal chemistry does not establish equal manufacturing, cleanliness, carbide distribution or finished-tool performance.
Why choose SHH STEEL for L2
SHH STEEL produces and exports L2 plate to a stated specification rather than an unqualified trade-name cross-reference. We review the product form, condition, machining allowance and inspection requirements before confirming the enquiry.
- Keep chemical limits and optional resulfurized variants explicit.
- Separate annealed acceptance from prescribed hardening response and final tool properties.
- Use plate/flat dimensional rules appropriate to the actual finish.
- Maintain heat identification and the required inspection reports.
Enquiry and inspection planning for L2
| Enquiry item | What to specify |
|---|---|
| Type / edition | L2 and the required ASTM edition |
| Form and dimensions | Plate or flat; thickness × width × length, quantity and finish |
| Condition | Annealed (197 BHN max on the reference basis) or separately specified treated state |
| Chemistry variant | Normal chemistry or explicitly specified resulfurized variant; required analysis reporting |
| Toolmaking | Intended die duty, final tool condition and any additional carbide/microstructure requirement |
| Inspection | Chemistry, hardness, test response, surface/decarburization and macrostructure acceptance |
| Documentation | Required test reports, heat identification and purchaser-witness provisions |
| Logistics | Destination, timing, packing and machining allowance |
Additional NDT or stricter quality requirements need agreed methods and acceptance criteria. A requested dimension or process is reviewed for feasibility; this page is not an unconditional stock or capacity commitment.
FAQ
-
What distinguishes L2 from other special-purpose grades?
- Table 1 allows carbon 0.45–1.00 %, but the Table 3 minimum response applies only to the 0.45–0.55 % carbon type under footnote A. Do not extend the low-carbon specimen response to the full chemistry window. Agree the selected carbon basis and applicable hardness/treatment acceptance before ordering.
-
Does the Table 3 HRC value describe annealed plate?
- No. Annealed acceptance is 2 BHN maximum in Table 2. The 53 HRC (0.45–0.55 % carbon type only; Table 3 footnote A) value is minimum hardening response on the prescribed specimen after the Table 3 treatment; it is not a universal final-die or as-delivered hardness.
-
Are the Table 3 temperatures a production heat-treatment guarantee?
- No. They are stipulated for the response test. The listed preheat (where specified), salt/furnace temperatures, quench medium and tempering duration define that test regime; the actual values are listed in the delivery section. Actual tool treatment depends on section and application.
-
Do these chemical limits allow an extra product-analysis tolerance?
- No. Table 1 note A says its limits include product-analysis tolerances. Normal P/S maxima and the Ni+Cu rule must be respected; optional sulfur requires an explicitly specified variant. Maximum-only limits are not required minimum additions; ellipses do not mean zero residual content.
-
Is the cited JIS or ISO name automatically equivalent?
- Lower-carbon application contrast only. The ASTM response footnote does not make this JIS grade an L2 equivalent. JIS SKS4 C 0.45–0.55 and W 0.50–1.00 versus the full L2 C 0.45–1.00 window and no specified W range. JIS Cr 0.50–1.00 versus L2 0.70–1.20. Match product form, full chemistry, hardness/test regime and inspection before any substitution.
Request a quotation
Request a quotation for ASTM A681 L2 tool steel plate or flat stock. Send the required edition, quantity, thickness, width and length, finish and machining allowance. Describe the die or tooling duty and identify whether the requirement is annealed machining stock or a separately specified hardened-and-tempered condition.
Include the hardness acceptance basis, hardening-response requirement and any additional macrostructure, carbide-quality, decarburization or NDT criteria. If a resulfurized variant is required, state that explicitly with the chemical and machining requirements. Provide the intended final tool properties separately rather than treating a specimen test as a production guarantee.
Send the inspection-report and heat-traceability requirements, destination, target delivery timing and packing needs. For a proposed foreign substitute, attach the governing specification and drawing so chemical, form and test differences can be reviewed before confirming the quotation.
For cut pieces, include the cutting drawing, grain-orientation needs, edge preparation and inspection stage. Confirm whether supplied dimensions are raw blanks or finished dimensions before order acceptance.
For L2, specify the selected carbon basis. The Table 3 response applies only to the 0.45–0.55 % carbon type; identify the applicable acceptance basis for other selections.