ASTM A681 H23 Tool Steel Plate | ASTM A681 Tool Steel - SHH STEEL

ASTM A681 H23 Tool Steel Plate

ASTM A681 H23 is high-chromium high-tungsten hot-work tool steel for hot extrusion inserts and thermal wear-loaded tooling. Its carbon range is 0.25–0.35 %, with alloy limits that distinguish it from neighboring die steels. Plate and flat blanks are selected by chemistry, delivery condition, surface quality and heat-treatment response rather than by a generic tool-steel nickname. Final tooling performance also depends on section, cooling and the qualified temper. SHH STEEL produces and exports H23 plate to the specified edition, dimensions and inspection requirements.
Equivalent Grades:
SKD5: hot-work contrast, not an established counterpart; chemistry and condition require review.
Heat Treatment
Annealed; hardened and tempered as specified.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
Conclusion

What is ASTM A681 H23 plate?

ASTM A681 H23 Tool Steel Plate is high-chromium high-tungsten hot-work tool steel. Chromium and tungsten are both 11.00–12.75 %, unlike the much lower-chromium H21 family. A specialized high-alloy hot-work route requiring the H23 balance rather than a generic tungsten die-steel name.

Numerical requirements here follow the finalized ASTM A681-08 (2008) text, approved 1 October 2008. This is a dated published-standard reference, not a claim that a later edition has identical tables. Plate, sheet, strip, bars and forgings are expressly within the wrought-product scope.

High alloy loading can favor resistance to thermal softening but complicate toughness and processing; qualify tool support, thermal cycling and final condition.

SHH STEEL produces and exports H23 plate against the agreed grade, condition and inspection basis. See ASTM A681 within Tool and Die Steel Plates.

Material specification for H23

Parameter Requirement / scope
Standard / type ASTM A681-08; H23, UNS T20823; hot-work tool steel
Product scope Available wrought products including hot/cold finished bar, plate, sheet, strip, rod, wire and forgings
Manufacture Electric melting unless otherwise specified; ingot/slab reduction sufficient to refine solidification structure, clause 5.1
Condition State annealed, hardened and tempered, or other specified condition under ordering clause 4.1.6
Chemistry Table 1 heat analysis; listed limits already include product-analysis tolerances
Annealed hardness Table 2: 255 BHN maximum
Cold-drawn hardness Table 2: 269 BHN maximum for that condition; not an annealed plate limit
Hardening response Table 3: minimum 42 HRC on the prescribed test specimen and treatment
Lot Each shipment of a heat by type, size and shape is a lot, clause 12.1
Unit basis Inch-pound values govern; parenthetical SI values are informational conversions, clause 1.3

Chemical composition of H23

Table 1 values below are mass percent. Listed limits already include product-analysis tolerances; do not add a separate allowance. An ellipsis means no listed limit for that element here, not a zero-content guarantee.

Element A681-08 Table 1 chemical requirement (wt. %)
Carbon (C) 0.25–0.35
Manganese (Mn) 0.15–0.40
Phosphorus (P) 0.030 max
Sulfur (S) 0.030 max
Silicon (Si) 0.15–0.60
Chromium (Cr) 11.00–12.75
Vanadium (V) 0.75–1.25
Tungsten (W) 11.00–12.75
Molybdenum (Mo) Not specified in Table 1

Unless otherwise specified, nickel plus copper shall not exceed 0.75 % (Table 1 note A). Where specified, sulfur may be 0.06–0.15 % to improve machinability (note D); this optional resulfurized route is distinct from the normal 0.030 % sulfur maximum. Heat analysis is required under clause 6.1. Clause 6.2 purchaser analysis is specifically described for finished bars/forgings; it is not a substitute plate sampling method or permission to widen the limits.

Hardness and minimum hardening response for H23

Table 2 gives H23 maximum annealed hardness of 255 BHN and a separate cold-drawn maximum of 269 BHN. Clause 7.1 refers to ASTM A370 and equivalent Rockwell values. The condition matters: a cold-drawn-flat limit is not automatically the limit for annealed plate.

Property / regime Value Meaning
Annealed acceptance 255 BHN max Specified annealed condition, Table 2
Cold-drawn acceptance 269 BHN max Only that delivery condition, Table 2
Minimum response to hardening 42 HRC Table 3 specimen response after stipulated treatment, not an as-delivered annealed hardness
Production tool properties Defined by the tool specification A test response does not guarantee arbitrary plate-section or finished-die properties

Clause 7.2 uses 1/4-in. (6.4-mm) thick disks representing the full cross section or the position midway between center and outer surface. Where form/size is unsuitable, longitudinal specimens may be used; these are at least 3 in. (76 mm) long with parallel flats ground on the original mill surfaces. Clause 7.2.1 uses the average of at least five hardness readings in the stated location, with light-load tests agreed where needed for thin pieces.

Delivery condition and response-test treatment for H23

Specify the delivery condition. An enquiry for annealed machining stock is different from one for hardened-and-tempered material. Table 2 calls the condition annealed; this edition does not impose a blanket spheroidizing temperature or a universal spheroidized-carbide rating. Specify any additional carbide-morphology requirement separately.

A681-08 Table 3 response-test item Reference
Preheat 1500 °F (816 °C)
Salt-bath austenitizing 2275 °F (1246 °C)
Controlled-atmosphere austenitizing 2300 °F (1260 °C)
Listed austenitizing time 5–15 min; apply Table 3 note 2 for furnace/salt method
Quench medium Oil
Temper 1200 °F (649 °C); double temper, 2 h each cycle
Minimum test response 42 HRC

Table 3 note 1 restricts these austenitizing temperatures to the response-to-hardening test; other combinations may be used for particular applications. Note 2 permits preheat ±25 °F (14 °C), but austenitizing/tempering ±10 °F (5.6 °C). Controlled-atmosphere specimens are held 5–15 min after reaching temperature; salt treatment follows the minimum time indicated. These are test-piece parameters, not a guaranteed production cycle for every plate thickness.

Welding, cutting and grinding H23

H23 is an alloy tool steel, not a readily weldable general fabrication plate. Tool repair welding requires a procedure matched to chemistry, prior condition, section, restraint and the intended final heat treatment. No generic preheat or post-weld temperature is prescribed here.

Thermal cutting, electrical discharge machining and grinding can leave altered layers or local cracking at the tool surface. Allow for finishing and inspect critical edges before final service. Grinding burn and tensile surface stresses can defeat an otherwise suitable die chemistry. High alloy loading can favor resistance to thermal softening but complicate toughness and processing; qualify tool support, thermal cycling and final condition.

Plate/flat dimensions, surface quality and inspection

Clause 10.1 invokes the applicable dimensional tables. Hot-rolled sheet/plate has its own Table 24 thickness tolerances and machining allowances, Table 25 trimmed width/length tolerances, Table 26 flatness and Table 27 camber. Flat bar or machined stock must use its applicable form-specific table rather than a round-bar diameter tolerance.

As a Table 24 example, hot-rolled plate over 0.500 through 1.000 in. (12.7–25.4 mm) has a 0.100-in. (2.54-mm) thickness tolerance, all over the specified thickness, and a 0.063-in. (1.60-mm) machining allowance. The table notes relate maximum decarburization to 80 % of the machining allowance per side and permit additional cleanup for flatness. This example is a tolerance reference, not a stock or capacity range.

Under clause 9.2, ground/polished, ground-finished or machine-finished material must be free of scale and decarburization. For other finishes, apply the appropriate size/shape limits and agree any tighter acceptance. Macrostructure is examined under clause 8/ASTM A561 for harmful porosity, segregation, inclusions, pipe and cracks; apply the appropriate composition/size rating, not an invented universal plate class.

Applications and selection limits for H23

Engineering applications considered for H23 include hot extrusion inserts and thermal wear-loaded tooling. A specialized high-alloy hot-work route requiring the H23 balance rather than a generic tungsten die-steel name. The standard classifies composition; the exact finished die, duty cycle and heat treatment still require engineering qualification.

Chromium and tungsten are both 11.00–12.75 %, unlike the much lower-chromium H21 family.

High alloy loading can favor resistance to thermal softening but complicate toughness and processing; qualify tool support, thermal cycling and final condition. Corrosion protection and thermal management are separate design matters; hot-work tool steel is not a pressure-vessel or stainless-service specification.

Compare H23 with published tool and engineering plates

The following own pages are already published. These are material-selection contrasts, not substitutes; tool performance cannot be inferred from carbon content or a shared plate form.

Material Type / chemistry Condition Property basis Typical route Substitution limit
H23 (this plate) high-chromium high-tungsten hot-work tool steel Annealed 255 BHN max; other condition specified Minimum response 42 HRC on Table 3 specimen Hot-work dies/tool inserts Not a carbon cutting-tool or machinery-alloy substitute
JIS G4401 SK140 Tool Steel Plate Carbon tool steel; published C 1.30–1.50 % As-hot-rolled unless otherwise specified; annealed/cold-rolled by agreement JIS G4401:2009 plate/strip hardness basis; not A681 Table 3 Cutting/file or edge-tool blanks as appropriate High-carbon cutting-tool route; lacks this specified tool-steel alloy balance
JIS G4401 SK120 Tool Steel Plate Carbon tool steel; published C 1.15–1.25 % As-hot-rolled unless otherwise specified; annealed/cold-rolled by agreement JIS G4401:2009 plate/strip hardness basis; not A681 Table 3 Cutting/file or edge-tool blanks as appropriate High-carbon cutting-tool route; lacks this specified tool-steel alloy balance
ASTM A829 4140 Alloy Steel Plate Cr-Mo engineering plate; published reference C 0.36–0.44 % Ordered condition on existing page Chemistry-ordered plate; no automatic A681 tool-hardness/response package Machinery parts and later heat-treated components Structural-quality engineering alloy, not an A681 matching tool-steel specification

International comparisons and substitution limits for H23

The JIS comparison below uses finalized JIS G 4404:2015 Table 5. Values in each pair are JIS first, ASTM second; all are wt. %. The ISO name, where present, is the JIS informational Annex JA.1 association, not a direct ASTM-certified equivalent.

Country / system Designation Actual differences / form Condition and substitution limit
United States ASTM A681-08 H23, UNS T20823 This wrought tool-steel specification, including plate Table 2 condition-specific hardness and Table 3 test response apply
Japan JIS G 4404:2015 SKD5 JIS SKD5 Cr 2.50–3.20 and W 8.50–9.50 versus H23 Cr 11.00–12.75 and W 11.00–12.75. Contrast only, not a dedicated counterpart; the JIS 2015 symbol is marked deletion at next revision. JIS annealed delivery, plate/flat acceptance and test regimes differ. The cited JIS sulfur limit is not automatically the ASTM limit.
International / European ISO route X30WCrV9-3 JIS Annex JA.1 informational comparison only; no complete ISO chemical window is asserted identical Confirm actual ISO edition, product form, heat-treatment and acceptance requirements; no direct DIN/ASTM alias is inferred

A681 Table 3 measures minimum response to hardening; JIS G4404 Table 10 and G4403 Table 7 HV values instead define practical-decarburization depth. Those regimes are not interchangeable. Similar principal chemistry does not establish equal manufacturing, cleanliness, carbide distribution or finished-tool performance.

Why choose SHH STEEL for H23

SHH STEEL produces and exports H23 plate to a stated specification rather than an unqualified trade-name cross-reference. We review the product form, condition, machining allowance and inspection requirements before confirming the enquiry.

  • Keep chemical limits and optional resulfurized variants explicit.
  • Separate annealed acceptance from prescribed hardening response and final tool properties.
  • Use plate/flat dimensional rules appropriate to the actual finish.
  • Maintain heat identification and the required inspection reports.

Enquiry and inspection planning for H23

Enquiry item What to specify
Type / edition H23 and the required ASTM edition
Form and dimensions Plate or flat; thickness × width × length, quantity and finish
Condition Annealed (255 BHN max on the reference basis) or separately specified treated state
Chemistry variant Normal chemistry or explicitly specified resulfurized variant; required analysis reporting
Toolmaking Intended die duty, final tool condition and any additional carbide/microstructure requirement
Inspection Chemistry, hardness, test response, surface/decarburization and macrostructure acceptance
Documentation Required test reports, heat identification and purchaser-witness provisions
Logistics Destination, timing, packing and machining allowance

Additional NDT or stricter quality requirements need agreed methods and acceptance criteria. A requested dimension or process is reviewed for feasibility; this page is not an unconditional stock or capacity commitment.

Request a quotation

Request a quotation for ASTM A681 H23 tool steel plate or flat stock. Send the required edition, quantity, thickness, width and length, finish and machining allowance. Describe the die or tooling duty and identify whether the requirement is annealed machining stock or a separately specified hardened-and-tempered condition.

Include the hardness acceptance basis, hardening-response requirement and any additional macrostructure, carbide-quality, decarburization or NDT criteria. If a resulfurized variant is required, state that explicitly with the chemical and machining requirements. Provide the intended final tool properties separately rather than treating a specimen test as a production guarantee.

Send the inspection-report and heat-traceability requirements, destination, target delivery timing and packing needs. For a proposed foreign substitute, attach the governing specification and drawing so chemical, form and test differences can be reviewed before confirming the quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X