A678 Grade A steel plate is a quenched-and-tempered structural-quality plate grade under ASTM A678/A678M-05(2009), Standard Specification for Quenched-and-Tempered Carbon and High-Strength Low-Alloy Structural Steel Plates (Withdrawn 2010). This page is written to that last edition. The specification was withdrawn in 2010, and no replacement edition is identified. This page does not claim current ASTM compliance. In the last edition, Grade A has a minimum yield strength of 50 ksi [345 MPa], a tensile strength of 70–90 ksi [485–620 MPa], a minimum elongation of 22% in 2 in. [50 mm], and a maximum thickness of 1½ in [40 mm]. For plates wider than 24 in. [600 mm], that elongation requirement is reduced by two percentage points. Confirm every figure against the official last-edition text if an order is placed to that withdrawn edition. SHH STEEL produces and exports ASTM A678 Grade A steel plate to the last-edition requirements on request.
Grade
A678 Grade A
Last edition
ASTM A678/A678M-05(2009)
Yield / tensile
50 ksi [345 MPa] min; 70–90 ksi [485–620 MPa]
Elongation, min
22% in 2 in. [50 mm]; reduced by 2 points for width over 24 in. [600 mm]
Max. thickness
1½ in [40 mm]
Condition
Quenched and tempered
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of ASTM A678 Grade A Steel Plate

ASTM A678/A678M-05(2009) covers quenched-and-tempered carbon steel and high-strength low-alloy steel plates of structural quality for welded, riveted, or bolted construction. Four grades — A, B, C and D — are listed in the official Scope of the last edition. ASTM A678 Grade A Steel Plate is Grade A of that edition. The specification was withdrawn in 2010; this page does not claim current ASTM compliance. General requirements on this page are those of the last edition as given in the official Scope. Confirm the official text of ASTM A678/A678M-05(2009).

ASTM A678 Grade A Steel Plate Material Specification

This page is written to the last edition, ASTM A678/A678M-05(2009). That specification was withdrawn in 2010, and no replacement edition is identified. Data on this page are those of that last edition. This page does not claim current ASTM compliance. Buyers should confirm every figure against the official text of ASTM A678/A678M-05(2009) if an order is placed to that withdrawn edition, and should confirm with the project engineer whether a current alternative specification is required.

ASTM A678 Grade A Steel Plate is described by ASTM A678/A678M-05(2009). The official title is “Standard Specification for Quenched-and-Tempered Carbon and High-Strength Low-Alloy Structural Steel Plates”.

The official Scope covers quenched-and-tempered carbon steel and high-strength low-alloy steel plates of structural quality for welded, riveted, or bolted construction. Inch-pound units and SI units are each to be regarded separately as standard; SI values are shown in brackets and are not exact equivalents, so each system is to be used independently of the other.

Plates furnished to the last edition shall conform to the applicable requirements of the general-requirements specification it references, ASTM A6/A6M, unless a conflict exists, in which case ASTM A678/A678M-05(2009) prevails. Fine austenitic grain size requirements of that referenced specification shall be met.

ASTM A678 Grade A Steel Plate Chemical Composition

Heat-analysis limits in the table are those of the last edition, ASTM A678/A678M-05(2009), which was withdrawn in 2010. Product analysis, if required, shall also conform to that edition. Thickness rows that the last edition does not describe for this grade are omitted. Confirm every figure against the official last-edition text if composition is required on the order.

Element Heat analysis, %
Carbon, max 0.16
Manganese, 1½ in. [40 mm] and under 0.90–1.50
Phosphorus, max 0.035
Sulfur, max 0.040
Silicon 0.15–0.50
Vanadium No requirement
Columbium (niobium) No requirement
Nitrogen No requirement
Copper, min, when specified 0.20

Small amounts of alloying elements may be present but shall not exceed: Cu 0.35%, Ni 0.25%, Cr 0.25%, Mo 0.08%. Boron may be added only by agreement between the producer and the purchaser. Grade A is specified only to a maximum thickness of 1½ in. [40 mm]. Thicker bands in the last-edition manganese table are not described for this grade and are omitted.

ASTM A678 Grade A Steel Plate Mechanical Properties

The official Scope of ASTM A678/A678M-05(2009), clause 1.3, lists the four grades. For Grade A on this page, that Scope gives a minimum yield strength of 50 ksi [345 MPa] min, a tensile strength of 70–90 ksi [485–620 MPa], and a maximum thickness of 1½ in [40 mm]. Table 1 of the last edition, reproduced below, gives the same Grade A yield and tensile values in every thickness band that edition describes for this grade, and adds the specified elongation. A size and grade marked “Not described” is not described in that edition and shall not be ordered as that combination.

Requirement Grade A Grade B Grade C Grade D
Yield strength, min, ksi [MPa] (0.2% offset or 0.5% extension under load)
To ¾ in. [20 mm], incl 50 [345] 60 [415] 75 [515] 75 [515]
Over ¾ to 1½ in. [20 to 40 mm], incl 50 [345] 60 [415] 70 [485] 75 [515]
Over 1½ to 2 in. [40 to 50 mm], incl Not described 60 [415] 65 [450] 75 [515]
Over 2 to 2½ in. [50 to 65 mm], incl Not described 60 [415] Not described 75 [515]
Over 2½ to 3 in. [65 to 75 mm], incl Not described Not described Not described 75 [515]
Tensile strength, ksi [MPa]
To ¾ in. [20 mm], incl 70–90 [485–620] 80–100 [550–690] 95–115 [655–790] 90–110 [620–760]
Over ¾ to 1½ in. [20 to 40 mm], incl 70–90 [485–620] 80–100 [550–690] 90–110 [620–760] 90–110 [620–760]
Over 1½ to 2 in. [40 to 50 mm], incl Not described 80–100 [550–690] 85–105 [585–720] 90–110 [620–760]
Over 2 to 2½ in. [50 to 65 mm], incl Not described 80–100 [550–690] Not described 90–110 [620–760]
Over 2½ to 3 in. [65 to 75 mm], incl Not described Not described Not described 90–110 [620–760]
Elongation in 2 in. [50 mm], min, % 22 22 19 18

Elongation in the table is the minimum in 2 in. [50 mm]. For Grade A that minimum is 22%. For thicknesses of ¾ in. [20 mm] and under, elongation is measured on a 1½-in. [40-mm] wide full-thickness rectangular specimen, in a 2-in. [50-mm] gage length that includes the fracture and shows the greatest elongation. For plates wider than 24 in. [600 mm], the elongation requirement is reduced by two percentage points, as provided by the general-requirements specification referenced by the last edition.

The last edition requires a tension test. One tension test shall be taken from a corner of each plate as heat treated. A Charpy V-notch impact test is a supplementary requirement and applies only when it is specified on the order. This page does not invent impact-energy values. Confirm every mechanical requirement against the official last-edition text if an order is placed to that withdrawn edition.

ASTM A678 Grade A Steel Plate Delivery Conditions

Plates under the last edition are quenched and tempered. The last edition requires heat treatment by heating to a temperature that produces an austenitic structure, but not exceeding 1700 °F [925 °C], holding a sufficient time to attain uniform heat throughout the material, quenching in a suitable medium, and tempering at not less than 1100 °F [593 °C]. The heat-treatment temperatures shall be reported in the test report. Do not assume an as-rolled or normalized delivery as a default of this grade. The last edition also requires the fine austenitic grain size requirements of the general-requirements specification it references.

Order information should include ASTM A678/A678M-05(2009) (the withdrawn last edition), the grade (Grade A), the dimensions and the quantity, the unit system (inch-pound or SI), and any agreed supplementary requirements. State clearly that the order is to a withdrawn specification if that is what the project requires, or state a current alternative if the engineer so directs. The official last-edition text and the inspection document govern acceptance of any supply to that edition.

ASTM A678 Grade A Steel Plate Weldability

The official Scope of the last edition states that, if the steel is to be welded, it is presupposed that a welding procedure suitable for the grade of steel and intended use or service will be used. This page does not invent a carbon equivalent, a preheat, or a qualified joint for Grade A. Procedure qualification is a project-engineering matter. Confirm the official welding wording and any project welding specification.

ASTM A678 Grade A Steel Plate Tolerances

Dimensional and mass tolerances for plates to this specification are those of the general-requirements specification referenced by the last edition, ASTM A6/A6M, unless a conflict exists, in which case ASTM A678/A678M-05(2009) prevails. This page does not tabulate those general tolerance values, because they belong to that referenced specification and depend on the ordered dimensions. Confirm the official last-edition text, the referenced general-requirements edition named on the order, and the ordered dimensions.

The official maximum thickness for Grade A is 1½ in [40 mm]. Thickness, width and length on the order shall not be assumed from this page alone.

ASTM A678 Grade A Steel Plate Applications and service limits

ASTM A678 Grade A Steel Plate is a quenched-and-tempered structural-quality plate for welded, riveted, or bolted construction, as described in the official Scope of the last edition. Selection of the grade, the thickness and the delivery condition is a design decision for the project engineer. The last edition does not, in the official Scope, assign a minimum design temperature, a pressure-equipment duty, a fire rating or a fatigue class. Because the specification was withdrawn in 2010, fitness for a current project shall be confirmed against the project specification; this page does not claim current ASTM compliance.

Compare A678 Grade A with other A678 grades and current alternatives

Grade A under ASTM A678/A678M-05(2009) is not a substitute for another A678 grade, and a similar yield strength in a current specification is not automatic equivalence. The last edition was withdrawn in 2010; current alternatives below are offered as alternatives, never as a claim of current ASTM A678 compliance. Figures for A678 Grades A–D are from the official last-edition Scope 1.3 and Table 1. Numeric cells for current alternatives are left blank of strength figures because those values belong to the named current specification and are not a claim of equivalence. Engineer approval is required before any substitution.

Designation Relationship Yield strength, min, ksi [MPa] Tensile strength, ksi [MPa] Maximum thickness, in. [mm] Note
A678 Grade A This page 50 [345] 70–90 [485–620] 1½ [40] Official last-edition Scope 1.3 and Table 1. Written to ASTM A678/A678M-05(2009) (Withdrawn 2010). Not current ASTM compliance. Not interchangeable with another A678 grade.
A678 Grade B Related A678 grade (not interchangeable) 60 [415] 80–100 [550–690] 2½ [65] Official last-edition Scope 1.3 and Table 1. Written to ASTM A678/A678M-05(2009) (Withdrawn 2010). Not current ASTM compliance. Not interchangeable with another A678 grade.
A678 Grade C Related A678 grade (not interchangeable) 75 [515] to ¾ in.; 70 [485] over ¾ to 1½ in.; 65 [450] over 1½ to 2 in. 95–115 [655–790] to ¾ in.; 90–110 [620–760] over ¾ to 1½ in.; 85–105 [585–720] over 1½ to 2 in. 2 [50] Official last-edition Table 1 (yield and tensile vary with thickness; maximum thickness 2 in. [50 mm]). Written to ASTM A678/A678M-05(2009) (Withdrawn 2010). Not current ASTM compliance. Not interchangeable with another A678 grade.
A678 Grade D Related A678 grade (not interchangeable) 75 [515] 90–110 [620–760] 3 [75] Official last-edition Scope 1.3 and Table 1. Written to ASTM A678/A678M-05(2009) (Withdrawn 2010). Not current ASTM compliance. Not interchangeable with another A678 grade.
ASTM A572 Grade 50 Current alternative topic — — — Current 50 ksi structural-plate grade that is not a quenched-and-tempered specification. Not an automatic equivalent of Grade A. Engineer approval is required before any substitution. Confirm both official texts.
EN 10025-6 Current alternative topic — — — Current quenched-and-tempered structural-plate family. Not an automatic equivalent of Grade A. Engineer approval is required before any substitution. Confirm both official texts.
ASTM A572 Current alternative topic — — — Current structural-plate family on this site. Not an automatic equivalent of Grade A. Engineer approval is required before any substitution. Confirm both official texts.
ASTM A633 Current alternative topic — — — Current normalized high-strength low-alloy structural-plate family on this site. Not an automatic equivalent of Grade A. Engineer approval is required before any substitution. Confirm both official texts.

ASTM A678 Grade A Steel Plate Equivalent Material Grade

The heading identifies a comparison topic, not a declaration of interchangeable material. No formal equivalence has been verified, and none of the rows below is automatic interchangeability. The last edition of A678 was withdrawn in 2010; current specifications named below are alternatives, not a continuation of ASTM A678.

Standard Country-Region Equivalent Grade Note
ASTM A678/A678M-05(2009) United States Grade A Quenched-and-tempered structural-quality plate on this page, written to the last edition (Withdrawn 2010). Not current ASTM compliance. Not interchangeable with another A678 grade.
EN 10025-6 Europe EN 10025-6 family Current quenched-and-tempered structural-plate family, commonly considered as a current alternative topic. Not an automatic equivalent. Engineer approval is required before any substitution.
ASTM A572/A572M United States A572 Grade 50 Current alternative (a current 50 ksi grade that is not a quenched-and-tempered specification). Not an automatic equivalent. Engineer approval is required before any substitution.

None of those relationships is interchangeability. Confirm every requirement against the official text of each standard named on the order, and obtain engineer approval before any substitution.

Why choose Us

SHH STEEL produces and exports structural steel plate, including enquiry support for ASTM A678 Grade A Steel Plate to the last edition, ASTM A678/A678M-05(2009), when a project still calls up that withdrawn specification. We review the ordered edition, the grade, the dimensions and the inspection plan, and we state clearly that ASTM A678 was withdrawn in 2010. We do not present supply as current ASTM A678 compliance, and we do not treat a current alternative as an A678 grade by default.

See the ASTM A678/A678M hub for the product family, and confirm whether the project requires the withdrawn last edition or a current alternative.

Our Service

To enquire, state ASTM A678/A678M-05(2009), the grade (Grade A), the product form and dimensions, the quantity, the unit system, and any agreed supplementary requirements. State whether the project requires the withdrawn last edition or a current alternative. SHH STEEL will confirm the inspection plan against the official last-edition text if that edition is ordered, and will not claim current ASTM compliance for a withdrawn specification. The official standard named on the order and the inspection document govern acceptance.

FAQ

What is A678 Grade A steel plate?

ASTM A678 Grade A Steel Plate is a quenched-and-tempered structural-quality plate grade under ASTM A678/A678M-05(2009), the last edition, which was withdrawn in 2010. This page is written to that last edition and does not claim current ASTM compliance. Grade A has a minimum yield strength of 50 ksi [345 MPa] min, a tensile strength of 70–90 ksi [485–620 MPa], a minimum elongation of 22% in 2 in. [50 mm], and a maximum thickness of 1½ in [40 mm]. For plates wider than 24 in. [600 mm], that elongation requirement is reduced by two percentage points. Confirm those figures against the official last-edition text.

Was ASTM A678 withdrawn, and is A678 Grade A still current?

Yes. ASTM A678/A678M-05(2009) was withdrawn in 2010, and no replacement edition is identified. This page is written to that last edition and does not claim current ASTM compliance. If a project still calls up A678, confirm the official last-edition text and the project specification, and consider a current alternative only with engineer approval. Current alternative families on this site include ASTM A572, ASTM A633 and EN 10025-6. Engineer approval is required before any substitution.

How does A678 Grade A differ from Grades B, C and D?

In ASTM A678/A678M-05(2009), Grade A has a minimum yield of 50 ksi [345 MPa], tensile 70–90 ksi [485–620 MPa], elongation 22% min in 2 in. [50 mm], and a maximum thickness of 1½ in [40 mm]. Grade B has a minimum yield of 60 ksi [415 MPa], tensile 80–100 ksi [550–690 MPa], elongation 22% min in 2 in. [50 mm], and a maximum thickness of 2½ in [65 mm]. Grade C has yield and tensile that vary with thickness in Table 1 (75 ksi [515 MPa] / 95–115 ksi [655–790 MPa] to ¾ in.; 70 ksi [485 MPa] / 90–110 ksi [620–760 MPa] over ¾ to 1½ in.; 65 ksi [450 MPa] / 85–105 ksi [585–720 MPa] over 1½ to 2 in.), elongation 19% min in 2 in. [50 mm], and a maximum thickness of 2 in [50 mm]. Grade D has a minimum yield of 75 ksi [515 MPa], tensile 90–110 ksi [620–760 MPa], elongation 18% min in 2 in. [50 mm], and a maximum thickness of 3 in [75 mm]. The four grades are not interchangeable. For plates wider than 24 in. [600 mm], the elongation requirement of the last edition is reduced by two percentage points. Confirm every figure against the official last-edition text.

What is the chemical composition of A678 Grade A?

Heat-analysis limits of ASTM A678/A678M-05(2009) for Grade A include carbon 0.16% max, manganese 0.90–1.50% in thicknesses 1½ in. [40 mm] and under, phosphorus 0.035% max, sulfur 0.040% max, silicon 0.15–0.50%, and copper 0.20% min when specified. The last edition states no requirement for vanadium, columbium (niobium) or nitrogen in Grade A. Residual copper, nickel, chromium and molybdenum shall not exceed 0.35%, 0.25%, 0.25% and 0.08% respectively. Boron may be added only by agreement. Confirm every figure against the official last-edition text. This page is written to the withdrawn last edition and does not claim current ASTM compliance.

How should A678 Grade A steel plate be ordered?

State ASTM A678/A678M-05(2009) if the withdrawn last edition is what the project requires, or state a current alternative if the engineer so directs, and the grade (Grade A). State the dimensions, the quantity and the unit system. This page does not claim current ASTM compliance. The official text of the specification named on the order governs acceptance.

Enquire about ASTM A678 Grade A Steel Plate

Enquire for ASTM A678 Grade A Steel Plate to ASTM A678/A678M-05(2009) (Withdrawn 2010), or for a current alternative if the project engineer so directs. State the grade (Grade A), the dimensions and the quantity. SHH STEEL will confirm the inspection plan against the official last-edition text if that edition is ordered. This page does not claim current ASTM compliance. The official standard and the inspection document govern acceptance.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X