New Products /back


13CrMoSi5-5,13CrMoSi5-5 steel plate,EN10028-2

2011年4月14日 by admin

EN10028-2,13CrMoSi5-5,13CrMoSi5-5,13CrMoSi5-5,13CrMoSi5-5

 

Adopt Standard: EN10028-2

Grade:P235GH,P265GH,P295GH,P355GH,16Mo3,18MnMo4-5,20MnMoNi4-5,15NiCuMoNb5-6-4,20MnMoNi4-5,15NiCuMoNb5-6-4,13CrMo4-5,13CrMoSi5-5,10CrMo9-10,12CrMo9-10,X12CrMo5,13CrMoV9-10,12CrMoV12-10,X10CrMoVNb9-1.

 

13CrMoSi5-5 steel grade

13CrMoSi5-5 steel grade is one of grade in En10028-2, which is non alloy and alloy steels with specified elevated temperature properties.

In accordance with en10020, 13CrMoSi5-5 steel grade is alloy special steels.

13CrMoSi5-5 Grade delivery condition is normalized and tempered or quenched and tempered.

 

Gangsteel could supply 13CrMoSi5-5 steel grade in super thick steel plate for fabricators serving the oil and gas industry, heat exchangers, weldable pressure vessels and boilers

For more information in 13CrMoSi5-5 steel grade in the following:


13CrMoSi5-5 Chemical composition cast analysis

Element

13CrMoSi5-5  Max %

Element

13CrMoSi5-5 max %

C

0.17

Cr

1.00-1.50

Si

0.50-0.80

Cu

0.30

Mn

0.40-0.65

Mo

0.45-0.65

P

0.015

Nb

 

S

0.005

Ni

0.30

AL

 

Ti

 

N

0.012

V

 

 

13CrMoSi5-5 Mechanical properties

Grade

Condition

Thickness

Yield Strength

Tensile Strength

Elongation

Impact Energy

(mm)

MPa (min)

MPa

% (min)

(KV J) (min)

 

 

 

 

-20 degree

13CrMoSi5-5

+NT or +QT

≤ 16

310

510-690

20

27

16> to ≤40

  310

510-690

20

27

40> to ≤60

310

480-660

20

27

60> to ≤100

310

500-680

20

27

100> to ≤150

310

490-670

20

27

150> to ≤250

310

490-670

20

27

Noted: +NT mean Normalized and tempered; +QT mean Quenched and tempered

 

If you want to find our stock in 13CrMoSi5-5 or inquiry from our gangsteel, please feel free to contact us by email or calling.

 

Tags: EN10028-2  13CrMoSi5-5  13CrMoSi5-5 steel  13CrMoSi5-5  13CrMoSi5-5  

0 Comments, 0 Trackbacks