Adopt Standard: EN10028-2

Grade:P235GH,P265GH,P295GH,P355GH,16Mo3,18MnMo4-5,20MnMoNi4-5,15NiCuMoNb5-6-4,20MnMoNi4-5,15NiCuMoNb5-6-4,13CrMo4-5,13CrMoSi5-5,10CrMo9-10,12CrMo9-10,X12CrMo5,13CrMoV9-10,12CrMoV12-10,X10CrMoVNb9-1.

 

10CrMo9-10 steel grade

10CrMo9-10 steel grade is one of grade in En10028-2, which is non alloy and alloy steels with specified elevated temperature properties.

In accordance with en10020, 10CrMo9-10 steel grade is alloy special steels.

10CrMo9-10 Grade delivery condition is normalized and tempered or quenched and tempered.

 

Gangsteel could supply 10CrMo9-10 steel grade in super thick steel plate for fabricators serving the oil and gas industry, heat exchangers, weldable pressure vessels and boilers

For more information in 10CrMo9-10 steel grade in the following:


10CrMo9-10 Chemical composition cast analysis

Element

10CrMo9-10  Max %

Element

10CrMo9-10 max %

C

0.08-0.14

Cr

2.00-2.50

Si

0.50

Cu

0.30

Mn

0.40-0.80

Mo

0.90-1.10

P

0.020

Nb

 

S

0.010

Ni

 

AL

 

Ti

 

N

0.012

V

 

 

10CrMo9-10 Mechanical properties

Grade

Condition

Thickness

Yield Strength

Tensile Strength

Elongation

Impact Energy

(mm)

MPa (min)

MPa

% (min)

(KV J) (min)

 

 

 

 

+20 degree

10CrMo9-10

+NT or +QT

≤ 16

310

480-630

18

31

16> to ≤40

  300

480-630

18

31

40> to ≤60

290

480-630

18

31

60> to ≤100

280

470-620

17

27

100> to ≤150

260

460-610

17

27

150> to ≤250

250

450-600

17

27

Noted: +NT mean Normalized and tempered; +QT mean Quenched and tempered

 