JIS G 3101:2024 SS400 steel bars use the bar mechanicals in Table 4, not the plate and section values in Table 3. Carbon and manganese are not specified for SS400; phosphorus and sulfur are 0.050 % maximum. Round sizes and unit masses follow JIS G 3191:2022 Tables 1 and 7, with each mass checked against the standard formula.
Keywords
SS400 steel bars, JIS G 3101 SS400, SS400 round bar, G 3191 bars, carbon steel bars
Equivalent Grades:
Near-equivalents only, not automatic substitutes.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Size Chart
Applications
Equivalent Grades
Sourcing
FAQ
Conclusion

What are JIS G 3101 SS400 Steel Bars?

JIS G 3101:2024 SS400 is a rolled steel for general structure. The type is applicable to steel plates, sheets, strips, sections and bars; this page is the bar product only. Mechanical properties for bars are taken from Table 4 of G 3101, which is not Table 3 (that table is for plates, sheets, strips, flats and sections). Using an SS400 I-beam or H-beam data sheet as a bar certificate would mix those tables.

Dimensions, calculated mass and permissible variations for hot-rolled bars and bar-in-coil are set by JIS G 3191:2022, which G 3101 lists among its normative references. The round-bar area and unit-mass table in that standard is Table 7, computed from the method in Table 6.

Material, Dimensions and Scope for JIS G 3101 SS400 Steel Bars

Heat analysis follows Table 2 of G 3101:2024. For SS400, carbon and manganese are not specified; phosphorus and sulfur are each 0.050 % maximum. Other elements may be added as permitted by the footnote to Table 2. Yield, tensile strength, elongation and bend properties for bars depend on the diameter or distance across flats, as set out in Table 4, with rounds measured by diameter and squares or hexagons by distance across flats.

G 3191:2022, clause 5.1, states that the standard diameters of cut (straight) round bars are 9 mm and above, and that bar-in-coil standard diameters are 50 mm and under. Diameters below 9 mm in Table 7 are therefore coil diameters, not cut-bar standard diameters. Parenthetical diameters in Tables 1 and 7 are permitted, but the standard prefers the diameters written without parentheses.

JIS G 3101 SS400 Chemical Composition (Heat Analysis)

Table 2 of JIS G 3101:2024 is short for SS400. There is no specified carbon or manganese maximum. Phosphorus is 0.050 % maximum and sulfur is 0.050 % maximum. That is a different rule from ASTM A36, which specifies carbon by thickness band and, above 3/4 in., a manganese range. It is also different from SS540 in the same Japanese standard, which does specify carbon and manganese.

Swipe horizontally to view all dimensions.

Element SS400 (Table 2, heat analysis)
Carbon Not specified
Manganese Not specified
Phosphorus, max 0.050 %
Sulfur, max 0.050 %

JIS G 3101 SS400 Steel Bar Mechanical Properties (Table 4)

Table 4 is the bar table. The tensile strength of SS400 is 400–510 N/mm² (MPa) in every diameter band. The minimum yield or proof strength is 245 N/mm² at 16 mm and under, 235 N/mm² over 16 mm up to 40 mm, 215 N/mm² over 40 mm up to 100 mm, and 205 N/mm² over 100 mm. Unless otherwise specified, the yield figure is the upper yield (ReH); if no yield point appears, Rp0.2 is measured.

Elongation is 20 % minimum on a No. 2 test piece for diameter or distance across flats of 25 mm and under, and 22 % minimum on a No. 14A test piece for sizes over 25 mm. The bend test is 180° around an inside radius of 1.5 times the diameter or distance across flats, using a No. 2 test piece, and the outside of the bent specimen shall be free from cracks. Do not apply the Table 3 (plate and section) elongation or bend radii to bars.

Swipe horizontally to view all dimensions.

Diameter or distance across flats Yield or proof, min, N/mm² Tensile strength, N/mm² Elongation, min Bend
16 mm and under 245 400–510 20 % (No. 2, ≤ 25 mm) 180°, radius 1.5 × size, No. 2 piece
Over 16 mm to 40 mm 235 400–510 20 % (No. 2) or 22 % (No. 14A, > 25 mm) Same bend rule
Over 40 mm to 100 mm 215 400–510 22 % (No. 14A, > 25 mm) Same bend rule
Over 100 mm 205 400–510 22 % (No. 14A) Same bend rule

JIS G 3101 SS400 Round Bar Sizes: JIS G 3191:2022 Table 7

The table below is the complete JIS G 3191:2022 Table 7 list of standard round diameters, cross-sectional areas and unit masses. Area is D² × 0.7854 mm², rounded to four significant figures; unit mass is 7.85 × 10⁻³ kg/(mm²·m) times that area, rounded to three significant figures, as required by Table 6. Every published mass on this page has been recomputed from that method and agrees with Table 7. Parenthetical diameters are permitted but not preferred. Cut-bar standard diameters start at 9 mm; 5.5–8 mm are bar-in-coil standard diameters. Squares and hexagons, if ordered, use the Table 6 formulae (A² and B² × 0.8660) rather than Table 7.

Swipe horizontally to view all dimensions.

Diameter, mm Preferred standard diameter Area, mm² Unit mass, kg/m
5.5 Yes 23.76 0.186
6 Yes 28.27 0.222
7 Yes 38.48 0.302
8 Yes 50.27 0.395
9 Yes 63.62 0.499
10 Yes 78.54 0.617
11 Yes 95.03 0.746
12 Yes 113.1 0.888
13 Yes 132.7 1.04
(14) Permitted (parenthetical) 153.9 1.21
16 Yes 201.1 1.58
(18) Permitted (parenthetical) 254.5 2
19 Yes 283.5 2.23
20 Yes 314.2 2.47
22 Yes 380.1 2.98
24 Yes 452.4 3.55
25 Yes 490.9 3.85
(27) Permitted (parenthetical) 572.6 4.49
28 Yes 615.8 4.83
30 Yes 706.9 5.55
32 Yes 804.2 6.31
(33) Permitted (parenthetical) 855.3 6.71
36 Yes 1018 7.99
38 Yes 1134 8.9
(39) Permitted (parenthetical) 1195 9.38
42 Yes 1385 10.9
(45) Permitted (parenthetical) 1590 12.5
46 Yes 1662 13
48 Yes 1810 14.2
50 Yes 1964 15.4
(52) Permitted (parenthetical) 2124 16.7
55 Yes 2376 18.7
56 Yes 2463 19.3
60 Yes 2827 22.2
64 Yes 3217 25.3
65 Yes 3318 26
(68) Permitted (parenthetical) 3632 28.5
70 Yes 3848 30.2
75 Yes 4418 34.7
80 Yes 5027 39.5
85 Yes 5675 44.5
90 Yes 6362 49.9
95 Yes 7088 55.6
100 Yes 7854 61.7
110 Yes 9503 74.6
120 Yes 11310 88.8
130 Yes 13270 104
140 Yes 15390 121
150 Yes 17670 139
160 Yes 20110 158
180 Yes 25450 200
200 Yes 31420 247

Applications and Service Limits for JIS G 3101 SS400 Steel Bars

SS400 bars are general-structure carbon steel, used for frames, fixtures, pins and miscellaneous fabrication where the order names G 3101 SS400. They are not a machine-steel grade, not a reinforcing-bar grade (those follow JIS G 3112), and not a pressure-vessel grade. Mass tolerance, when the purchaser requires it, follows G 3191:2022 Table 8 and is applied to a group of the same size, not to a single short length by default.

Near-Equivalents for JIS G 3101 SS400 Steel Bars: Not Automatic Substitutes

ASTM A36 bars and EN 10025-2 S235JR bars are the usual comparisons, because the yield bands overlap in the thinner sizes. They are not automatic substitutes. A36 specifies carbon by thickness and a 58–80 ksi tensile range; SS400 does not specify carbon and uses a 400–510 N/mm² tensile range with Japanese test-piece numbers. SS400 sections use Table 3, not Table 4, so an SS400 I-beam page is not this product.

GB/T 700 Q235B is another frequent comparison and is likewise a starting point for a study, not a restamping rule. Confirm the product form, the mechanical table, and the dimensional standard actually named on the order.

Sourcing JIS G 3101 SS400 Steel Bars from SHH STEEL

SHH STEEL reviews enquiries for JIS G 3101 SS400 bars against the G 3101 edition, the product form (cut bar or bar-in-coil), the diameter or distance across flats, the length, and the certificate. Table 7 is the standard round-size list, not a catalogue of guaranteed mill items. If a square or hexagon, a mass-tolerance certificate to Table 8, or a comparison with A36 is required, that should be written on the enquiry.

JIS G 3101 SS400 Steel Bar FAQs

Is Table 3 or Table 4 used for SS400 bars?
Table 4. Table 3 is for plates, sheets, strips, flats and sections. Elongation test pieces and bend radii are not the same in the two tables.
Does SS400 specify carbon?
No. Table 2 of G 3101:2024 leaves carbon and manganese unspecified for SS400. Phosphorus and sulfur are each 0.050 % maximum.
Are diameters below 9 mm standard cut bars?
No. G 3191:2022 clause 5.1 sets cut-bar standard diameters at 9 mm and above. Diameters 5.5–8 mm in Table 7 are standard diameters for bar-in-coil.
How were the unit masses checked?
Each Table 7 mass was recomputed as 7.85 × 10⁻³ times the tabulated area (itself D² × 0.7854, four significant figures), rounded to three significant figures as required by Table 6.

Conclusion

JIS G 3101:2024 SS400 bars are general-structure carbon steel with Table 4 mechanicals, unspecified carbon and manganese, and 0.050 % maximum phosphorus and sulfur. Round sizes on this page are the complete JIS G 3191:2022 Table 7 list, with formula-checked unit masses; cut-bar standard diameters start at 9 mm. Do not use an SS400 section table, or an A36 bar table, as a substitute certificate. Name the form, the diameter and the editions on the order.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X