CNS 7851 SY295 U-Type Steel Sheet Pile

CNS 7851 SY295 U-type steel sheet pile is a Taiwanese hot-rolled interlocking U-section with a 295 N/mm² minimum yield and a 490 N/mm² minimum tensile strength. The page also covers SY390, lists a verified 400 × 170 × 15.5 mm mill designation, and distinguishes the different JIS A 5528 tensile minima.
Keywords
CNS 7851 SY295 U-Type Steel Sheet Pile, SY295 sheet pile, SY390, CNS 7851, U-type 400 × 170
Equivalent Grades:
SY390 (same standard, higher yield); JIS A 5528 SY295/SY390 (same SY names, different tensile minima); JIS A 5523 SYW — comparisons only, not automatic substitutes.
Share:
General Description
Material Specification
Available Sizes of CNS 7851 SY295 U-Type Steel Sheet Pile
Chemical Composition of CNS 7851 SY295 and SY390
Mechanical Properties of CNS 7851 SY295 and SY390
Shape Tolerances and Identification
Delivery Conditions, Inspection and Identification
Applications and Service Limits
CNS 7851 Compared with JIS A 5528 and JIS A 5523
Near-Equivalents: Not Automatic Substitutes
Sourcing CNS 7851 SY295 U-Type Steel Sheet Piles from SHH STEEL
FAQ
Conclusion

What is CNS 7851 SY295 U-Type Steel Sheet Pile?

CNS 7851 SY295 U-type steel sheet pile is a hot-rolled interlocking U-section whose material grade is SY295 under CNS 7851, with SY390 listed on the same page as the higher-yield quality in the same standard. SY marks a steel sheet pile, and 295 is the minimum yield stress in N/mm². In CNS 7851:2018 the minimum tensile strength of SY295 is 490 N/mm², with a minimum elongation of 18%. SY390 has a minimum yield of 390 N/mm², a minimum tensile strength of 540 N/mm² and a minimum elongation of 16%.

This page covers the CNS 7851 family in U-type form. The Japanese sister standard of the same SY names is JIS A 5528 SY295 U-type steel sheet pile; those tensile minima are not the CNS figures and must not be mixed on a certificate. These piles are filed under the steel sheet piles category in the steel structural profiles catalog. They are not H-beams, channels, or bearing piles, and a 400 mm U-type designation is not a Chinese or European U pile of similar width.

Material, Dimensions and the SY295 / SY390 Family

The purchase order and the inspection document should name, separately:

  • CNS 7851 and its edition (this page uses the 2018 edition as reprinted for these grades; the edition named on the order governs), and the grade SY295 or SY390;
  • the U-type geometry (for example 400 × 170 × 15.5 mm) and the required length;
  • any agreed chemistry, impact test, coating or interlock check that is not in the tabulated mill reprint.

CNS 7851 is not JIS A 5528 and is not JIS A 5523.

CNS 7851 SY295 U-Type Size: 400 × 170 × 15.5 mm Mill Designation

The table below is one published mill U-type designation, 400 × 170 × 15.5 mm, which has the same geometry as JIS Type IV. It is not a complete CNS 7851 size table. Other U-type sections can be reviewed when they are named on the enquiry and certified to CNS 7851. A 400 mm U-type pile is not a Chinese or European U pile of similar width.

Effective width and height are the interlocking-wall dimensions used for this section. Mass per metre of wall is the published figure for a continuous wall of this effective width, not a claim that every wall is built from this section alone.

Swipe horizontally to view all dimensions.

Geometry Effective width (mm) Effective height (mm) Thickness (mm) Section area (cm²) Second moment of area (cm⁴) Section modulus (cm³) Mass (kg/m) Wall area (cm²/m) Wall second moment (cm⁴/m) Wall section modulus (cm³/m) Wall mass (kg/m²)
U-type 400 × 170 × 15.5 (JIS Type IV geometry) 400 170 15.5 96.99 4,670 362 76.1 242.5 38,600 2,270 190

CNS 7851 Chemical Composition

The figures below are the chemistry reprint for CNS 7851:2018 SY295 and SY390 on the same mill page as the 400 × 170 × 15.5 mm U-type section. Carbon, silicon, manganese, nitrogen and carbon equivalent are not specified in that table. Phosphorus and sulphur are each 0.04% maximum. Do not invent a carbon or manganese limit, and do not read a Ceq from another sheet-pile standard onto this certificate.

Grade C Si Mn P S N Ceq
SY295 Not specified Not specified Not specified 0.04 max 0.04 max Not specified Not specified
SY390 Not specified Not specified Not specified 0.04 max 0.04 max Not specified Not specified

CNS 7851 Mechanical Properties

The tensile values below are from the same CNS 7851:2018 reprint. There is no tabulated Charpy V-notch energy at 0 °C in that table. If an impact test is required, it must be agreed and written on the order.

Grade Min. yield (N/mm²) Min. tensile (N/mm²) Min. elongation (%) Absorbed energy at 0 °C (J)
SY295 295 min 490 min 18 min Not specified
SY390 390 min 540 min 16 min Not specified

U-Type Shape Tolerances and Identification

The tolerances below are the U-type shape and dimension tolerances published with this mill designation. If the ordered edition of CNS 7851 gives different limits, the ordered edition governs.

Item Condition U-type tolerance
Width — +10 mm / −5 mm
Height — ± 4%
Thickness t < 10 mm ± 1.0 mm
Thickness 10 mm ≤ t < 16 mm ± 1.2 mm
Thickness t ≥ 16 mm ± 1.5 mm
Length — + unlimited / −0
Camber, parallel to the wall Length ≤ 10 m Not more than the length in metres × 0.12%
Camber, parallel to the wall Length > 10 m Not more than [(length − 10 m) × 0.10% + 12 mm]
Sweep, perpendicular to the wall Length ≤ 10 m Not more than the length in metres × 0.25%
Sweep, perpendicular to the wall Length > 10 m Not more than [(length − 10 m) × 0.20% + 25 mm]
Out-of-square at a cut end — Not more than 4% of the width

A typical inspection mark identifies the steel standard and grade, the dimension number, the heat number, the producer, the length and the manufacturing number. An SY295 certificate is not an SY390 certificate, and a JIS A 5528 mark is not a CNS 7851 mark.

Delivery Conditions, Inspection and Identification

These piles are commonly supplied as-rolled. The inspection document should identify CNS 7851 and its edition, the grade SY295 or SY390, the U-type geometry, the length, the heat analysis for the elements reported, and the tensile results. A JIS A 5528 certificate, a plate certificate, or an H-beam certificate does not, by itself, identify a CNS 7851 U-type sheet pile.

Applications and Service Limits

CNS 7851 SY295 and SY390 U-type piles are used in retaining walls, cofferdams, quay work and similar interlocking-wall structures where a Taiwanese sheet-pile grade is named. They are not a silent substitute for JIS A 5528 SY295 U-type steel sheet pile, for a GB/T 20933 U-type section, or for a European U or Z pile. Interlocks of similar width are not interchangeable by depth or mass alone.

CNS 7851 Compared with JIS A 5528 and JIS A 5523

The comparisons below are an orientation only; they are not automatic substitutes.

Grade / designation Standard Relationship to CNS 7851 SY295 U-type pile Caution
CNS 7851 SY390 CNS 7851:2018 The higher-yield quality on this page, with a 390 N/mm² minimum yield and a 540 N/mm² minimum tensile strength. SY390 is not a silent upgrade of SY295, and it is not JIS A 5528 SY390.
JIS A 5528 SY295 / SY390 JIS A 5528:2021 Japanese designations of the same SY names, often compared on the same U-type section. JIS SY295 has a 450 N/mm² tensile minimum, not the CNS 490 N/mm² figure. See JIS A 5528 SY295 U-type steel sheet pile.
JIS A 5523 SYW295 / SYW390 JIS A 5523 Weldable hot-rolled sheet-pile grades sometimes compared with these SY names. SYW is a different standard. A CNS 7851 certificate is not an A 5523 certificate.

Near-Equivalents: Not Automatic Substitutes

A near-equivalent is a starting point for a discussion, not a licence to swap certificates. If a project names CNS 7851 SY295 or SY390, keep that standard, quality and designation on the order. The Japanese sister page is JIS A 5528 SY295 U-type steel sheet pile.

Sourcing CNS 7851 SY295 U-Type Steel Sheet Piles from SHH STEEL

SHH STEEL supplies CNS 7851 SY295 and SY390 U-type steel sheet piles against a named geometry, the material edition and the inspection document type. Enquiries should state the U-type geometry and length, the grade, whether JIS A 5528 SY295 U-type steel sheet pile is acceptable on part of the list, and any coating, corner piles or interlock requirements.

The size table is one published mill U-type designation, not a claim that every CNS sheet-pile section is rolled in every quality. Once the list is clear, a quotation can be prepared against the stated edition and certificate.

CNS 7851 SY295 U-Type Steel Sheet Pile FAQs

Is CNS 7851 SY295 the same as JIS A 5528 SY295?
No. The yield minima are the same 295 N/mm², but CNS 7851 SY295 has a 490 N/mm² tensile minimum and JIS A 5528 SY295 has a 450 N/mm² tensile minimum. The same difference appears on SY390 (540 versus 490 N/mm²). Certify to the standard named on the order.
Is 400 × 170 × 15.5 mm the complete CNS 7851 size table?
No. That geometry is one published mill U-type designation, the same geometry as JIS Type IV. Other U-type piles can be reviewed when they are named and certified to CNS 7851. It is not a Chinese or European U pile of similar width.
Does CNS 7851 SY295 have a standard 0 °C impact test?
The mill reprint used for this page does not tabulate a Charpy energy at 0 °C for SY295 or SY390. If an impact test is required, it should be agreed and written on the order.
Which edition of CNS 7851 is used on this page?
The numeric tables use the CNS 7851:2018 reprint published with this mill designation. A later edition may be named on the order; the ordered edition governs.

Request a Quotation for CNS 7851 SY295 U-Type Steel Sheet Pile

CNS 7851 SY295 U-type steel sheet pile is a hot-rolled interlocking U-section with a 295 N/mm² minimum yield and a 490 N/mm² minimum tensile strength. Nominate the U-type geometry (for example 400 × 170 × 15.5 mm), the grade SY295 or SY390, CNS 7851:2018 or the edition on the order, the length, and the inspection document type. Send the size list, grade, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X