CNS 13812 SN490B Steel Channel

CNS 13812 SN490B steel channel is a Taiwanese and Japanese building-structure channel in the 490–610 N/mm² tensile class, with a 27 J impact test at 0 °C. The page also covers SN400B, SN400YB and SN490YB, and lists the complete JIS G 3192 Table 12 channel series as reference dimensions.
Keywords
CNS 13812 SN490B Steel Channel, SN490B channel, SN400YB channel, SN490YB, JIS G 3136 channel
Equivalent Grades:
SN400YB/B and SN490YB (same family); SM490 — comparisons only, not automatic substitutes.
Share:
General Description
Material Specification
Available Sizes of SN490B Steel Channel
Chemical Composition of SN490B Steel Channel
Mechanical Properties of SN490B Steel Channel
Delivery Conditions, Inspection and Identification
Weldability of SN490B Steel Channels
Shape Tolerances and Theoretical Mass
Applications and Service Limits
SN490B Compared with SN400YB and SM490
Near-Equivalents: Not Automatic Substitutes
Sourcing SN490B Steel Channels from SHH STEEL
FAQ
Conclusion

What is CNS 13812 SN490B Steel Channel?

CNS 13812 SN490B steel channel is a hot-rolled building-structure channel whose material grade is SN490B under CNS 13812. The same SN family is specified in JIS G 3136:2022. SN marks a building-structure steel, 490 is the tensile-strength class (490–610 N/mm²), and B is the quality with a 27 J impact requirement at 0 °C when testing applies. Related qualities on this page are SN400B, SN400YB and SN490YB.

These bars are filed under steel channel profiles in the steel structural profiles category. The designation is H×B×t1×t2, for example 200×90×8×13. They are not GB/T 706 or European sections of a similar millimetre size, and they are not JIS G 3106 SM490 bars, even when the same JIS G 3192 size table is used.

Material, Dimensions and the SN Quality Family

The purchase order and the inspection document should name CNS 13812 or JIS G 3136 and its edition, the full quality symbol, the dimensional standard (CNS 1490 or JIS G 3192), the designation (H×B×t1×t2), and the inspection document type.

SN490B Steel Channel Sizes: JIS G 3192 Series

The table is the complete standard channel series in JIS G 3192:2024 Table 12: 16 sizes, from 75×40×5×7 to 380×100×13×20. The tabulated dimensions are representative; other section dimensions may be used by agreement. Name CNS 1490 or JIS G 3192 as the dimensional standard actually required. A published mill production band such as 25–100 mm is a mill range, not a complete standard table, and is not used here as a size list. Governing thickness for the material tables is ordinarily the flange t2.

Swipe horizontally to view all dimensions.

Designation (H×B×t1×t2) H (mm) B (mm) t1 (mm) t2 (mm) r1 (mm) r2 (mm) A (cm²) Mass (kg/m)
75×40×5×7 75 40 5 7 8 4 8.818 6.92
100×50×5×7.5 100 50 5 7.5 8 4 11.92 9.36
125×65×6×8 125 65 6 8 8 4 17.11 13.4
150×75×6.5×10 150 75 6.5 10 10 5 23.71 18.6
150×75×9×12.5 150 75 9 12.5 15 7.5 30.59 24.0
180×75×7×10.5 180 75 7 10.5 11 5.5 27.20 21.4
200×80×7.5×11 200 80 7.5 11 12 6 31.33 24.6
200×90×8×13.5 200 90 8 13.5 14 7 38.65 30.3
250×90×9×13 250 90 9 13 14 7 44.07 34.6
250×90×11×14.5 250 90 11 14.5 17 8.5 51.17 40.2
300×90×9×13 300 90 9 13 14 7 48.57 38.1
300×90×10×15.5 300 90 10 15.5 19 9.5 55.74 43.8
300×90×12×16 300 90 12 16 19 9.5 61.90 48.6
380×100×10.5×16 380 100 10.5 16 18 9 69.39 54.5
380×100×13×16.5 380 100 13 16.5 18 9 78.96 62.0
380×100×13×20 380 100 13 20 24 12 85.71 67.3

SN490B and Related SN Chemical Composition

The figures below are heat-analysis maxima as reprinted from CNS 13812 (JIS G 3136:2022). Boron is shown as less than 0.0008%. Carbon equivalent and Pcm are the tabulated maxima; the calculation in the ordered edition of the standard governs, and no formula is invented here. For SN490B the catalog reprints two Ceq maxima, 0.44 and 0.46, in two thickness bands; the 40 mm split is clear for SN490YB (0.44 then 0.46) and is not forced onto SN490B on this page. The edition named on the order governs the applicable band.

Swipe horizontally to view all dimensions.

Grade Thickness (mm) C max Si max Mn P max S max B max Ceq max Pcm max
SN400B 6 ≤ t ≤ 50 0.20 0.35 0.60–1.50 0.030 0.015 0.0008 0.36 0.26
SN400B 50 < t ≤ 100 0.22 0.35 0.60–1.50 0.030 0.015 0.0008 0.36 0.26
SN400YB 6 ≤ t ≤ 100 0.20 0.35 0.60–1.50 0.030 0.015 0.0008 0.36 0.26
SN490B 6 ≤ t ≤ 50 0.18 0.55 1.05 max 0.030 0.015 0.0008 0.44 / 0.46 (two bands; ordered edition governs the cut) 0.29
SN490B 50 < t ≤ 100 0.20 0.55 1.05 max 0.030 0.015 0.0008 0.44 / 0.46 (two bands; ordered edition governs the cut) 0.29
SN490YB 6 ≤ t ≤ 40 0.18 0.55 1.05 max 0.030 0.015 0.0008 0.44 0.29
SN490YB 40 < t ≤ 100 0.18 0.55 1.05 max 0.030 0.015 0.0008 0.46 0.29

SN490B Mechanical Properties: Yield, Tensile and 0 °C Impact

The mechanical values below are those reprinted for section steels with a flange thickness of 6 mm to 40 mm. They are not extended above 40 mm on this page. For H-sections with a web thinner than 9 mm, the upper yield limit in the range columns does not apply, and the yield-ratio maximum is 85% rather than 80%. Thickness for these tables is the flange thickness of the finished section unless the order names another location.

Annex rules for legs under 40 mm do not apply: every Table 12 channel has a flange width B of 40 mm or more.

Swipe horizontally to view all dimensions.

Grade Min. or range of yield, thinner bands (N/mm²) Yield at t = 16 mm and 16 < t ≤ 40 mm (N/mm²) Tensile strength (N/mm²) Max. yield ratio (%) Min. elongation, t ≥ 6 mm and t ≤ 16 mm (%) Min. elongation, 16 < t ≤ 40 mm (%) Impact, 0 °C (J)
SN400B ≥ 235 235–355 400–510 80 18 22 27
SN400YB ≥ 250 250–355 400–510 80 20 22 27
SN490B ≥ 325 325–445 490–610 80 17 21 27
SN490YB 325–445 325–445 490–610 80 17 21 27

Impact results are the mean of three tests at 0 °C, 27 J, for the B and YB qualities in this table.

Delivery Conditions, Inspection and Identification

The inspection document should identify CNS 13812 (or JIS G 3136) and its edition, the full quality symbol, the dimensional standard and designation, heat analysis, Ceq or Pcm, and tensile and impact results against the governing thickness. A plate or H-beam certificate does not, by itself, identify a steel channel.

Weldability of SN490B Steel Channels

SN steels are specified as building-structure steels with a published Ceq and Pcm. Preheat and consumable choice should use the certified heat analysis, the certified Ceq or Pcm, the actual thickness and the joint design.

CNS 1490 or JIS G 3192 Shape Tolerances and Theoretical Mass

Shape, mass and tolerances belong to the dimensional standard named on the order, ordinarily CNS 1490 or JIS G 3192. Mass in the size table is the published theoretical figure. Millimetre tolerance tables are not reproduced here.

Applications and Service Limits

SN490B steel channels are used in building frames and bracing where a Taiwanese or Japanese SN 490-class building-structure grade and a 0 °C impact test are specified. They are not a silent substitute for an SM490 channel or for a GB/T 706 or European section of similar size.

SN490B Compared with SN400YB and SM490

The comparisons below are an orientation only; they are not automatic substitutes.

Grade / designation Standard Relationship to SN490B steel channel Caution
SN400YB / SN400B / SN490YB CNS 13812; JIS G 3136:2022 Related SN qualities on this page. The tensile class, yield window and carbon table differ. Do not treat an SN400 certificate as SN490B.
SN400YB H-beam CNS 13812; dimensions JIS G 3192 Table 15 The same material family in H-section form. A channel or angle designation is not an H-section.
SM490 JIS G 3106; dimensions JIS G 3192 A Japanese welded-structure comparison, not an SN building-structure grade. See JIS G 3106 SM490 H-beam for the SM family in H-section form.

Near-Equivalents: Not Automatic Substitutes

A near-equivalent is a starting point for a discussion, not a licence to swap certificates. If a project names SN490B or SN490YB, keep that quality letter and the dimensional standard on the order.

Sourcing SN490B Steel Channels from SHH STEEL

SHH STEEL supplies CNS 13812 SN490B steel channels, and the related SN400 and SN490YB qualities, against a named designation list, the material edition and the inspection document type. Enquiries should state the H×B×t1×t2 designations, the quality letter, whether CNS 1490 or JIS G 3192 is required, cut lengths or mill lengths, and any processing.

The size table is the standard series, not a claim that every designation is rolled in every quality. Once the list is clear, a quotation can be prepared against the stated edition and certificate.

SN490B Steel Channel FAQs

Is SN490B the same as SN400YB or SM490?
No. SN490B is a 490 N/mm² tensile-class building-structure grade with a 0 °C / 27 J impact test. SN400YB is a 400 N/mm² class with a yield window. SM490 is a JIS G 3106 welded-structure grade, not an SN grade.
Do the mechanical tables apply above 40 mm?
The tabulated mechanical values on this page are those reprinted for finished sections with a flange or leg thickness of 6 mm to 40 mm. Values above 40 mm are not invented here.
Is a 25–100 mm mill band the complete size table?
No. A mill production band is not a standard series. This page lists the complete tabulated JIS G 3192 series as reference dimensions. The order should name the designations actually required.
Which material edition is used on this page?
The numeric tables follow the CNS 13812 / JIS G 3136:2022 reprint in the mill catalog used for this page. The edition named on the order governs.

Request a Quotation for CNS 13812 SN490B Steel Channel

CNS 13812 SN490B steel channel is a building-structure channel in the 490–610 N/mm² tensile class, with a 27 J impact requirement at 0 °C. Nominate the H×B×t1×t2 designation, the quality letter, CNS 13812 or JIS G 3136 and the dimensional standard on the order, and the inspection document type. Send the size list, quality, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X