BS 1501 321S51 Steel Plate | BS 1501 Steel - SHH STEEL

BS 1501 321S51 Steel Plate

BS 1501 321S51 is a higher-carbon titanium-stabilized chromium-nickel steel for plates, sheet and strip under BS 1501-3:1990. A public secondary extract shows carbon 0.04–0.10 %, chromium 17.00–19.00 % and nickel 9.00–12.00 %. The numeric titanium window was not printed and is not invented here. Solution-annealed material is listed with a 0.2 % proof stress of 175 MPa minimum. SHH STEEL produces and exports 321S51 plate to the ordered edition, delivery condition and dimensions.
Equivalent Grades:
Near names include AISI 321H and EN 10028-7 X6CrNiTi18-10 (1.4541); not automatic substitutes.
Heat Treatment
Solution annealed at 1020–1120 °C; supplied finally annealed.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is BS 1501 321S51 plate?

We produce and export BS 1501 321S51 as higher-carbon titanium-stabilized chromium-nickel steel for pressure purposes. Typical service is corrosion- or heat-resisting pressure equipment that specifies this steel number.

BS 1501-3:1990 is the last final edition of the corrosion- and heat-resisting plate, sheet and strip part of BS 1501. It was published on 28 February 1990 and superseded on 15 July 2000. It superseded BS 1501-3:1973. The replacement set includes BS EN 10028-7 for stainless flat products for pressure purposes, together with later dimensional standards such as BS EN 10029, BS EN 10048, BS EN 10051, BS EN 10258 and BS EN 10259. Clause 2 of the 1990 book is titled Designation, but that clause text was not opened. The steel numbers used here (for example 304S11) come from a public materials-database list of 21 BS 1501-3 materials and from the same secondary extract. The letter S is part of those British steel numbers. No extra A or B order suffix was sourced. These numbers are not BS 970 or BS 1502 bar grades and not BS 1449-2 general-purpose stainless grades (those books use some overlapping names, and different numbers such as 309S24).

A public catalogue abstract of BS 1501-3:1990 states that the part covers plates from 3 mm to 100 mm, sheet from 0.30 mm to less than 3 mm, and narrow strip from 0.050 mm to less than 3 mm, for ambient, elevated and low-temperature duty. The same abstract notes that, except for duplex 318S13, the listed steels are considered for ambient temperature and down to −196 °C. That scope note is recorded as an abstract, not as a photographed clause.

Numeric cells below are taken from a public secondary extract headed BS 1501/3-1990, opened on 8 November 2026 (Asia/Shanghai). The extract’s subjects match the official 1990 contents list: Table 1 covers cast analysis, ambient mechanical properties and heat treatment; Tables 13 and 14 cover elevated-temperature Rp0.2 and Rp1.0. Some HTML table tags were broken; manganese and molybdenum bounds were recovered from those broken cells (for example a silicon cell written as 1.00

2.00

for manganese 2.00). The two columns after manganese were headed only as dashes and sit in the conventional phosphorus and sulfur positions; they are labelled that way with this caveat. A photographed BSI PDF of BS 1501-3:1990 was not opened. These figures are a reference basis, not an official-complete 1990 guarantee and not an SHH proprietary guarantee. They are not copied from ASTM A240/ASME SA240 304-family tables or from BS 970 bar grades. A public materials-database listing labels 321S51 as CrNi 18/9 0.10C Ti. That qualitative titanium identity is recorded, but no numeric titanium cell is shown.

SHH STEEL produces and exports BS 1501 321S51 plate, sheet or strip to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for BS 1501 321S51

The items below follow BS 1501-3:1990 as the historical corrosion- and heat-resisting plate, sheet and strip book. Numeric cells in the chemical and mechanical sections come from the public secondary extract described there, not from a photographed 1990 Table 1. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard BS 1501-3:1990, Steels for pressure purposes — Specification for corrosion- and heat-resisting steels: plates, sheet and strip
Designation used here BS 1501 321S51 (steel number sourced from the opened 21-name list and the secondary extract; Clause 2 text unread)
Steel type Higher-carbon titanium-stabilized chromium-nickel steel
Product form Corrosion- and heat-resisting plate, sheet and strip for pressure purposes (this part does not cover bars, sections, tubes, forgings or carbon/alloy Part 1 and Part 2 plates)
How designations are listed Sourced steel numbers take the form 304S11, 316S13 and similar. The letter S is part of the British steel number. No extra A or B suffix was sourced. These are not BS 970 bar designations
Thickness mentioned in the opened abstract Abstract: plates 3 mm to 100 mm; sheet 0.30 mm to less than 3 mm; narrow strip 0.050 mm to less than 3 mm
Usual heat treatment Solution annealed at 1020–1120 °C; supplied finally annealed.
Chemical analysis Cast analysis cells from the opened secondary extract of the 1990 composition table, each labelled by source
Tensile properties Ambient Rp0.2, Rp1.0 and elongation from the opened secondary extract; the printed tensile window was held as defective; titanium % was not printed
Our supply We produce and export 321S51 plate, sheet or strip to the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of BS 1501 321S51

Numeric cells below are taken from a public secondary extract headed BS 1501/3-1990, opened on 8 November 2026 (Asia/Shanghai). The extract’s subjects match the official 1990 contents list: Table 1 covers cast analysis, ambient mechanical properties and heat treatment; Tables 13 and 14 cover elevated-temperature Rp0.2 and Rp1.0. Some HTML table tags were broken; manganese and molybdenum bounds were recovered from those broken cells (for example a silicon cell written as 1.00

2.00

for manganese 2.00). The two columns after manganese were headed only as dashes and sit in the conventional phosphorus and sulfur positions; they are labelled that way with this caveat. A photographed BSI PDF of BS 1501-3:1990 was not opened. These figures are a reference basis, not an official-complete 1990 guarantee and not an SHH proprietary guarantee. They are not copied from ASTM A240/ASME SA240 304-family tables or from BS 970 bar grades.

Element Value (wt. %) Source opened for this cell
Carbon (C) 0.04–0.10 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Silicon (Si) 1.00 (single printed figure in the Si column; treated here as a maximum) Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Manganese (Mn) 2.00 max (recovered from a broken HTML cell after silicon) Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Phosphorus (P) 0.045 max (dash-headed column after manganese) Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Sulfur (S) 0.025 max (dash-headed column after phosphorus) Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Chromium (Cr) 17.00–19.00 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Nickel (Ni) 9.00–12.00 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Titanium (Ti) Not printed on the opened extract; a numeric titanium window is not invented here Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)

Tensile and elevated-temperature properties for BS 1501 321S51

Ambient tensile properties and the listed solution-annealing range below come from the opened secondary extract of the 1990 combined chemistry/mechanical/heat-treatment table.

Item Value Source opened for this cell
0.2 % proof stress Rp0.2, MPa min 175 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
1.0 % proof stress Rp1.0, MPa min 210 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Tensile strength Rm, MPa Not published here as a usable specification cell (the extract printed a defective tensile window; see the caption) Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Elongation A, % min 35 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Solution-annealing temperature, °C 1020–1120 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
Intergranular-corrosion note on the extract Sensitization time 30 min when an intergranular-corrosion test is required (extract note 5). Note 7: as-rolled supply note does not apply; plate is supplied finally solution annealed Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)

Strength values are in MPa, equivalent to N/mm². On the extract, a disputed elongation test uses a proportional round specimen with gauge length 5.65 √So, or a 12.5 mm wide rectangular specimen with a 50 mm gauge length. The extract printed a tensile window of 190–690 MPa. That minimum is below the listed 1.0 % proof stress of 210 MPa and is treated as a defective cell, so no tensile-strength number is published here. Numeric cells below are taken from a public secondary extract headed BS 1501/3-1990, opened on 8 November 2026 (Asia/Shanghai). The extract’s subjects match the official 1990 contents list: Table 1 covers cast analysis, ambient mechanical properties and heat treatment; Tables 13 and 14 cover elevated-temperature Rp0.2 and Rp1.0. Some HTML table tags were broken; manganese and molybdenum bounds were recovered from those broken cells (for example a silicon cell written as 1.00

2.00

for manganese 2.00). The two columns after manganese were headed only as dashes and sit in the conventional phosphorus and sulfur positions; they are labelled that way with this caveat. A photographed BSI PDF of BS 1501-3:1990 was not opened. These figures are a reference basis, not an official-complete 1990 guarantee and not an SHH proprietary guarantee. They are not copied from ASTM A240/ASME SA240 304-family tables or from BS 970 bar grades.

Elevated-temperature minimum proof-stress values below come from the opened secondary extract whose subjects match official 1990 Tables 13 (Rp0.2) and 14 (Rp1.0). They are table values, not allowable design stresses and not a published maximum service temperature. In the elevated-temperature tables, some HTML tags were again broken (for example a cell written as 144

132

). Those missing opening tags were recovered in the same way as the manganese and molybdenum cells. The extract listed temperatures through 700 °C; values printed at 650 °C and 700 °C are shown when present. A dash means no figure was printed at that temperature.

Temperature Rp0.2, MPa min Rp1.0, MPa min Source
20 °C 175 210 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
100 °C 128 166 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
150 °C 123 155 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
200 °C 117 147 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
250 °C 114 141 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
300 °C 110 133 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
350 °C 105 129 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
400 °C 100 126 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
450 °C 95 121 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
500 °C 93 118 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
550 °C 90 116 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
600 °C 88 115 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
650 °C 86 112 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)
700 °C 84 108 Public secondary extract headed BS 1501/3-1990, opened 8 November 2026 (Asia/Shanghai)

Numeric cells below are taken from a public secondary extract headed BS 1501/3-1990, opened on 8 November 2026 (Asia/Shanghai). The extract’s subjects match the official 1990 contents list: Table 1 covers cast analysis, ambient mechanical properties and heat treatment; Tables 13 and 14 cover elevated-temperature Rp0.2 and Rp1.0. Some HTML table tags were broken; manganese and molybdenum bounds were recovered from those broken cells (for example a silicon cell written as 1.00

2.00

for manganese 2.00). The two columns after manganese were headed only as dashes and sit in the conventional phosphorus and sulfur positions; they are labelled that way with this caveat. A photographed BSI PDF of BS 1501-3:1990 was not opened. These figures are a reference basis, not an official-complete 1990 guarantee and not an SHH proprietary guarantee. They are not copied from ASTM A240/ASME SA240 304-family tables or from BS 970 bar grades.

Delivery conditions for BS 1501 321S51

The opened extract lists solution annealing at 1020–1120 °C and says the as-rolled supply note does not apply, so plate is supplied in the final solution-annealed condition. Name the required delivery condition on the purchase order.

On the opened extract, water cooling or rapid cooling in air is stated for the solution treatment, except where a note says that as-rolled supply after a sufficiently hot rolling practice does not apply and the plate is supplied in the final solution-annealed condition. For these steels the extract says annealing, solution treatment and solution annealing have the same meaning.

If the project has moved to EN 10028-7, order the successor designation and edition expressly. A later European name is not by itself a substitute instruction for 321S51.

The purchase order should name the official steel number, the edition required, whether plate, sheet or strip is wanted, thickness, width and length, the delivery condition, any intergranular-corrosion or elevated-temperature tests, and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

BS 1501-3:1990 does not itself set a welding procedure for 321S51 on the pages opened for this article. Welding and thermal cutting should be qualified for the alloy content, thickness and the specified solution-annealed delivery condition.

The higher listed carbon range is the identity of 321S51 compared with 321S31. The numeric titanium window was not printed and is not invented here. Consumables should match the qualified procedure for this higher-carbon titanium-stabilized family. Do not assume an AISI 321H or EN 10028-7 1.4541 welding procedure without a project review.

Heat input and any required post-weld treatment belong in the project specification. This page does not publish a pitting-resistance equivalent or a maximum service temperature.

Form, appearance, dimensions and thickness tolerances

Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate, and later sheet and strip tolerance standards, when those standards are specified.

Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.

Applications and specification limits

We produce and export 321S51 as corrosion- and heat-resisting steel plate, sheet and strip for pressure purposes. Typical service is pressure equipment that specifies the higher-carbon 321S51 number rather than 321S31.

BS 1501-3:1990 is a historical stainless flat-product standard. It is not the current EN 10028-7 order unless that successor standard is written on the enquiry, and it is not a BS 1501-1 carbon, BS 1501-2 alloy, BS 1502 bar or BS 1503 forging order.

Compare BS 1501 321S51 with other steel plates

BS 1501 321S51 is a historical BS 1501-3 corrosion- and heat-resisting flat product. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
BS 1501 321S51 (this plate) Higher-carbon Ti-stabilized Cr-Ni steel; C 0.04–0.10 %, Cr 17.00–19.00 %, Ni 9.00–12.00 %; Ti window not printed Solution annealed at 1020–1120 °C; supplied finally annealed. Extract: Rp0.2 175 MPa min; Rp1.0 210 MPa min; A 35 % min; tensile strength not published from the defective extract cell Corrosion- or heat-resisting pressure equipment that specifies this steel number A later EN 10028-7 or ASTM A240 name is not an automatic substitute
EN 10028-7 X6CrNiTi18-10 (1.4541) Later titanium-stabilized Cr-Ni pressure-vessel stainless plate Solution annealed (+AT) as specified in EN 10028-7 Live published Rp0.2 at least 200 MPa and Rm 500–700 MPa Modern European 321-family vessel plate Near name only; those EN tensile numbers are not copied onto 321S51
AISI 321H stainless steel plate Higher-carbon titanium-stabilized stainless plate on the live AISI page Solution annealed Live published yield at least 205 MPa and tensile at least 515 MPa Common mill 321H plate Different book and strength basis; not an automatic substitute
EN 10028-7 X6CrNi18-10 (1.4948) Later higher-carbon Cr-Ni pressure-vessel stainless plate without a titanium identity on that live page Solution annealed (+AT) as specified in EN 10028-7 Live published Rp0.2 at least 190 MPa and Rm 510–710 MPa Modern European 304H-family vessel plate Different stabilizer practice from 321S51

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. Confirm chemistry, including residuals such as nitrogen, titanium, niobium or copper where they apply, together with heat treatment, proof stress, tensile properties, intergranular-corrosion testing and product form. EN 10028-7 and ASTM A240/ASME SA240 are later books with their own tables.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United Kingdom BS 1501-3:1990 321S51 This plate. Extract Rp0.2 175 MPa minimum and Rp1.0 210 MPa minimum. The printed tensile window was held as defective. Titanium % was not printed. This product
United States AISI / ASTM A240 family (live AISI 321H page) 321H Live published yield at least 205 MPa and tensile at least 515 MPa. Related product form only
Europe EN 10028-7 X6CrNiTi18-10 (1.4541) Later titanium-stabilized vessel plate. Live published Rp0.2 200 MPa minimum and Rm 500–700 MPa. Near name only
China / other — — No separately verified GB plate counterpart was established as an automatic equivalent for 321S51 on this page. Do not assume a local 321H name is a substitute

Why choose SHH STEEL for BS 1501 321S51

  • We produce and export BS 1501 321S51 corrosion- and heat-resisting plate, sheet and strip
  • We review the enquiry for edition, steel number, delivery condition, product form, dimensions and extra tests
  • We keep the historical BS 1501-3 steel number distinct from later EN 10028-7 names, from ASTM A240/ASME SA240 types, and from BS 970 bar grades
  • We match documentation to what the purchase order requires

Our Service

Item What to specify
Standard and designation BS 1501 321S51 and the edition required (BS 1501-3:1990)
Or successor standard The EN 10028-7 steel name or number and edition, if that is what the project now requires
Delivery condition Solution annealed at 1020–1120 °C; supplied finally annealed.
Product form and dimensions Plate, sheet or strip, with required thickness, width and length
Chemistry Cast analysis to the named edition
Mechanical tests Proof stress, tensile strength, elongation and, where specified, intergranular-corrosion or elevated-temperature proof tests to the named edition
Other tests Ultrasonic examination or other extra tests only when written on the order
Documentation State the inspection document type required by the project

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

Frequently Asked Questions

Is BS 1501-3 still a current product standard?
No. BS 1501-3:1990 is the last final edition of the corrosion- and heat-resisting plate, sheet and strip part. It was published on 28 February 1990 and superseded on 15 July 2000. EN 10028-7 superseded part of it. Projects still using a historical steel number should name the edition required on the order.
Which numbers on this page are photographed 1990 table values?
None are presented as a photographed BSI PDF. Cast analysis, ambient tensile properties, solution-annealing temperatures and elevated proof-stress figures come from a public secondary extract headed BS 1501/3-1990. Some HTML tags were broken and were recovered as described in the tables. They are a reference basis, not an official-complete guarantee.
What does the S in a number such as 304S11 mean, and is there an A or B suffix?
The opened sources list complete steel numbers such as 304S11, 316S31 and 318S13. The letter S is part of that British steel number. Clause 2, Designation, was not opened, so further suffix rules are not stated here. No extra A or B order suffix was sourced. These numbers are not copied from BS 970 bar grades.
Why is no tensile-strength range shown for 321S51?
The opened extract printed 190–690 MPa. That minimum is below the listed 1.0 % proof stress of 210 MPa and is treated as a defective cell, so it is not published as a specification figure. Confirm tensile strength against the named edition.
What should a quotation enquiry include?
BS 1501 321S51, the edition required or the successor designation, whether plate, sheet or strip is wanted, the delivery condition, thickness by width by length, quantity, any intergranular-corrosion or elevated-temperature tests, and the inspection document required.

Request a quotation

Contact SHH STEEL for a quotation for BS 1501 321S51 plate, sheet or strip. Please include your required quantity, thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the edition (BS 1501-3:1990, or a named EN 10028-7 successor if that is what the project now requires), the delivery condition and any specimen heat treatment. If your project requires an intergranular-corrosion test, a stated elevated-temperature proof test, ultrasonic examination or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness. A later EN 10028-7 or ASTM A240 name is not by itself a substitute instruction.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response