ASTM B709 N08028 Alloy 28 Plate
What is ASTM B709 N08028 (Alloy 28) Plate?
As a stainless steel supplier and China mill-direct exporter, SHH STEEL supplies ASTM B709 UNS N08028 (Alloy 28) Plate. UNS N08028, commonly called Alloy 28, is an iron-nickel-chromium-molybdenum alloy with 30.0 – 34.0 % nickel, 26.0 – 28.0 % chromium, 3.0 – 4.0 % molybdenum and 0.6 – 1.4 % copper, with carbon limited to 0.030 %.
Its European counterpart is EN 10088-2 1.4563 plate. SHH STEEL supplies the standard grade N08028 unless a specific mill is named.
This page summarises the requirements for ASTM B709 N08028 plate and sheet: chemical composition, mechanical properties, heat treatment and the general delivery requirements of ASTM B906. Values are from ASTM B709-22 (published October 2022), which refers to ASTM B906 for general requirements. Check the edition named on your order. SHH STEEL confirms the edition named on the drawing before an order is placed.
N08028 material specification and SHH STEEL supply scope
| Item | Requirement | SHH STEEL supply |
|---|---|---|
| Standard | ASTM B709-22 / ASME SB-709, iron-nickel-chromium-molybdenum alloy (UNS N08028) plate, sheet and strip | Full compliance; edition confirmed at order |
| Grade | UNS N08028 | Confirmed by heat analysis on the certificate |
| General requirements | ASTM B906: dimensions, tolerances, testing and marking | Tolerances checked against ASTM B906 |
| Product forms | Plate, sheet and strip | Plate, sheet, strip and cut-to-size blanks |
| Delivery condition | Solution annealed | Written into the mill order |
| Inspection document | Mill test report per ASTM B906 | EN 10204 3.1 standard; 3.2 with third-party witness on request |
ASTM B709 refers to ASTM B906 for general requirements, including dimensions, tolerances, testing and certification. The ASME counterpart is SB-709.
Chemical composition of N08028 (ASTM B709, %)
| Element | Content (%) |
|---|---|
| Carbon (C) | ≤ 0.030 |
| Silicon (Si) | ≤ 1.00 |
| Manganese (Mn) | ≤ 2.50 |
| Phosphorus (P) | ≤ 0.030 |
| Sulphur (S) | ≤ 0.030 |
| Nickel (Ni) | 30.0 – 34.0 |
| Chromium (Cr) | 26.0 – 28.0 |
| Molybdenum (Mo) | 3.0 – 4.0 |
| Copper (Cu) | 0.6 – 1.4 |
| Iron (Fe) | Balance |
The high chromium and nickel, with molybdenum and copper, give resistance to sulphuric and phosphoric acid and to chloride stress corrosion cracking.
Mechanical properties of N08028 (ASTM B709)
| Property | Requirement |
|---|---|
| Tensile strength | ≥ 500 MPa |
| Yield strength (0.2 %) | ≥ 214 MPa |
| Elongation in 50 mm | ≥ 40 % |
| Hardness (for information) | 70 – 90 HRB |
The hardness range is given for information only and is not an acceptance requirement.
Heat treatment and delivery condition of N08028
| Item | Value (ASTM B709-22) |
|---|---|
| Final heat treatment | Solution anneal (clause 6.1); minor cold work such as flattening or temper rolling allowed afterwards |
| Recommended solution anneal (Note 1) | Heat to at least 1 080 °C (1 975 °F), cool rapidly to room temperature |
| General requirements | ASTM B906 |
SHH STEEL asks the mill to record the solution-annealing temperature on the certificate.
Lead time from the mill is normally 30 – 40 days after order confirmation, depending on size, finish and rolling schedule. Dimensional tolerances follow ASTM B906 unless the order states otherwise.
Key characteristics of Alloy 28 (N08028)
- Iron-nickel-chromium-molybdenum alloy with 30.0 – 34.0 % nickel and 26 – 28 % chromium.
- Copper 0.6 – 1.4 % for sulphuric acid resistance.
- Tensile strength ≥ 500 MPa, yield strength ≥ 214 MPa, elongation ≥ 40 %.
- Low carbon (≤ 0.030 %) for welded fabrication.
- Ordered by standard and UNS number: ASTM B709, UNS N08028.
N08028 equivalent grades
| System | Grade | Comment |
|---|---|---|
| EN 10088-2 | EN 10088-2 1.4563 plate | European counterpart (X1NiCrMoCu31-27-4) |
| ASTM, related | ASTM A240 Type 904L sheet and plate | Lower nickel and chromium; not equivalent |
For pressure equipment in Europe, see EN 10028-7 1.4563 pressure vessel plate. For a 6 % molybdenum alternative, EN 10088-2 1.4529 plate may be compared.
Applications of ASTM B709 UNS N08028 (Alloy 28) Plate
Euro Inox lists these typical applications for the EN equivalent 1.4563:
- Heat exchangers in contact with sulphuric and phosphoric acid contaminated by chlorides and fluorides
- Pipes in the oil and gas industry
- Equipment needing good resistance to pitting, crevice corrosion and stress corrosion cracking
Where conditions are less severe, EN 10088-2 1.4539 plate (904L) may be enough. SHH STEEL supplies Alloy 28 plate for these uses as full plates or cut-to-size blanks.
N08028 compared with related high-alloy grades
The table compares N08028 with the high-alloy austenitic grades most often considered for the same acid and chloride service. N08028 values are from ASTM B709-22 Tables 1 and 2; the others are from ASTM A240-22.
| Grade | Standard | Cr % | Ni % | Mo % | Cu % | N % | Tensile / yield min, MPa |
|---|---|---|---|---|---|---|---|
| ASTM A240 Type 904L (N08904) | ASTM A240 | 19.0 – 23.0 | 23.0 – 28.0 | 4.00 – 5.00 | 1.00 – 2.00 | ≤ 0.10 | 490 / 220 |
| S31254 | ASTM A240 | 19.5 – 20.5 | 17.5 – 18.5 | 6.0 – 6.5 | 0.50 – 1.00 | 0.18 – 0.25 | 655 / 310 |
| N08926 | ASTM A240 | 19.0 – 21.0 | 24.0 – 26.0 | 6.00 – 7.00 | 0.50 – 1.50 | 0.15 – 0.25 | 650 / 295 |
| N08028 | ASTM B709 | 26.0 – 28.0 | 30.0 – 34.0 | 3.0 – 4.0 | 0.6 – 1.4 | – | 500 / 214 |
N08028 has the highest chromium and nickel of these grades but less molybdenum than the 6 % Mo grades. In EN terms, 904L corresponds to EN 10088-2 1.4539, S31254 to EN 10088-2 1.4547 and N08926 to EN 10088-2 1.4529. SHH STEEL can quote these alloys side by side.
Corrosion resistance of N08028
Using PREN = %Cr + 3.3 × %Mo, the B709 limits give N08028 a PREN of about 35.9 at the minimum and 41.2 at the maximum (B709 sets no nitrogen range). Its strength lies in the combination of very high chromium and nickel with molybdenum and copper.
Euro Inox lists heat exchangers in contact with sulphuric and phosphoric acid contaminated by chlorides and fluorides, and oil and gas pipes, for the EN equivalent 1.4563, together with good resistance to pitting, crevice corrosion and stress corrosion cracking. The high nickel content is what gives the alloy its resistance to chloride stress corrosion cracking compared with the 300-series grades. B709 allows one corrosion test per lot when the purchaser specifies it; SHH STEEL writes the test method and acceptance into the order.
Physical properties of N08028
| Property | Typical value (Euro Inox, EN 1.4563) |
|---|---|
| Density | 8.0 g/cm³ |
| Modulus of elasticity at 20 °C | 195 GPa |
| Mean thermal expansion 20 – 200 °C | 16.1 × 10⁻⁶ /K |
| Mean thermal expansion 20 – 400 °C | 16.9 × 10⁻⁶ /K |
| Thermal conductivity at 20 °C | 12 W/(m·K) |
| Specific heat at 20 °C | 450 J/(kg·K) |
| Electrical resistivity at 20 °C | 1.00 Ω·mm²/m |
These are typical values for the EN equivalent and are not requirements of ASTM B709. The alloy is non-magnetic. On request, SHH STEEL can pass on the producing mill’s data sheet.
Welding, forming and machining N08028
N08028 is fully austenitic and is welded by the usual arc processes. For the EN equivalent 1.4563, Euro Inox lists nickel-base filler materials 2.4621, 2.4653 and 2.4656, which are more highly alloyed than the base metal so that the weld keeps its corrosion resistance. Carbon is limited to 0.030 %, which reduces the risk of carbide precipitation in the heat-affected zone.
The alloy forms well (elongation ≥ 40 %) but work-hardens, so forming forces rise with deformation and machining needs rigid set-ups, sharp tools and positive rake. B709 allows minor cold work such as flattening after the final solution anneal. SHH STEEL can supply N08028 plate cut to size with bevels for welding.
Testing, lots and tolerances under ASTM B709
- Lot (clause 10.1): one heat, same condition and thickness, solution annealed by the same practice, not more than 11 340 kg (25 000 lb).
- Number of tests (clause 11.1): for flat sheet, strip or plate, one tension test and one or more hardness tests per 100 pieces or less of the same lot; for coils, tension tests from each end of each coil.
- Corrosion test: one per lot when specified.
- Tension specimens (clause 12): full thickness, sheet-type under 12.7 mm and plate-type at 12.7 mm and over, to ASTM E8/E8M.
- Product (check) analysis to the requirements of ASTM B906 when made by the purchaser.
For sheet, B709 Table 3 limits flatness to 12.7 – 25.4 mm deviation depending on width and thickness, and Table 4 allows items of five sheets or less (or under 90.7 kg) to weigh up to 10 % over theoretical weight, and larger items up to 7.5 %. Plate follows the tolerances of ASTM B906. SHH STEEL checks that the certificate identifies the lot and reports all required tests.
How to order N08028 plate
- Specification: ASTM B709-22 or ASME SB-709, UNS N08028.
- Product form: plate, sheet or strip, with thickness, width, length and quantity.
- Condition: solution annealed (the only condition B709 covers).
- Any corrosion test, with method and acceptance.
- Inspection document (3.1 or 3.2) and third-party inspection if required.
- Dual certification to EN 10088-2 1.4563 if needed.
- Marking, packing and destination.
B709 clause 4 makes the purchaser responsible for specifying all requirements, with the ordering section of ASTM B906 as a guide. SHH STEEL reviews the enquiry against both standards before quoting.
N08028 (ASTM B709) and EN 1.4563 compared
| Element / property | ASTM B709-22 N08028 | EN 10088-2 1.4563 | Overlap for dual certification |
|---|---|---|---|
| C, max % | 0.030 | 0.020 | ≤ 0.020 |
| Si, max % | 1.00 | 0.70 | ≤ 0.70 |
| Mn, max % | 2.50 | 2.00 | ≤ 2.00 |
| S, max % | 0.030 | 0.010 | ≤ 0.010 |
| Ni % | 30.0 – 34.0 | 30.0 – 32.0 | 30.0 – 32.0 |
| Cr % | 26.0 – 28.0 | 26.0 – 28.0 | 26.0 – 28.0 |
| Mo % | 3.0 – 4.0 | 3.0 – 4.0 | 3.0 – 4.0 |
| Cu % | 0.6 – 1.4 | 0.70 – 1.50 | 0.70 – 1.40 |
| N, max % | not specified | 0.10 | ≤ 0.10 |
| Yield / tensile, MPa | ≥ 214 / ≥ 500 | ≥ 220 / 500 – 700 | ≥ 220 / 500 – 700 |
EN 10088-2 limits are tighter for carbon, silicon, manganese, sulphur and nickel, so a heat made to EN 1.4563 usually also meets B709, but the reverse is not automatic. EN 10088-2 lists 1.4563 as hot-rolled plate only, up to 75 mm, and adds requirements that B709 does not have: a minimum 1 % proof strength of 260 MPa (for guidance), Charpy V impact energy of at least 100 J longitudinal and 60 J transverse above 10 mm, and resistance to intergranular corrosion to EN ISO 3651-2 in both the delivery and the sensitized condition. A dual-certified certificate should report these as well. SHH STEEL checks both standards when a drawing names them together.
Proof strength of the EN equivalent at temperature
| Temperature, °C | 100 | 200 | 300 | 400 | 500 | 550 |
|---|---|---|---|---|---|---|
| Rp0.2 min, MPa (EN 1.4563) | 190 | 160 | 150 | 135 | 120 | 115 |
ASTM B709 gives room-temperature properties only. EN 10088-2 Table 12 gives minimum 0.2 % proof strength values for the EN equivalent 1.4563 from 100 to 550 °C, which can guide early design; code design must use the allowable stresses of the applicable code. SHH STEEL can provide the EN values with a dual-certified heat.
N08028 designations
UNS N08028 is the designation used by ASTM B709 and its ASME counterpart SB-709. The alloy type is widely known as Alloy 28. In Europe it is the stainless steel 1.4563 (X1NiCrMoCu31-27-4). B709 was originally approved in 1982. Purchase orders should name the specification and UNS number rather than any producer name. SHH STEEL quotes the standard grade and names a brand only when the customer asks for it.
Sheet flatness under ASTM B709 Table 3
| Thickness | Width | Maximum deviation from flat |
|---|---|---|
| 1.57 mm and over | up to 1 524 mm | 12.7 mm |
| 1.57 mm and over | 1 524 – 1 829 mm | 19.1 mm |
| 1.57 mm and over | over 1 829 mm | 25.4 mm |
| under 1.57 mm | up to 914 mm | 12.7 mm |
| under 1.57 mm | 914 – 1 524 mm | 19.1 mm |
| under 1.57 mm | over 1 524 mm | 25.4 mm |
These limits apply to sheet not specified as stretcher levelled. Where flatter sheet is needed, it should be stated on the order. SHH STEEL can arrange levelling and cut-to-length processing.
Cleaning N08028 after fabrication
Good practice for high-alloy stainless steels applies to N08028: iron transferred from carbon-steel tools or shop dust should be removed before service, by mechanical or chemical cleaning. ASTM A380 describes cleaning, descaling and passivation methods and ASTM A967 covers chemical passivation treatments and how to verify them. Weld spatter, heat tint, flux, slag and arc strikes can act as crevices in chloride service and should be removed, preferably by pickling or by fine grinding, since coarse grinding marks can trap deposits.
SHH STEEL supplies N08028 plate in the solution-annealed and pickled condition and can advise on surface protection during transport and fabrication.
What changed in ASTM B709-22
B709 was originally approved in 1982. The previous edition was B709-17, which had replaced B709-04 (2014). The 2022 edition (approved 1 October 2022, published October 2022) makes the product (check) analysis requirement refer to ASTM B906 instead of ASTM B880, adds ASTM B899 for terminology, and states that the general requirements are those of B906 rather than of its current edition; the redline shows no change to the Table 1 chemical limits or the Table 2 mechanical properties. Orders and certificates should name the edition. SHH STEEL quotes B709-22 unless the customer names an earlier edition.
Sampling after delivery and retests
Clause 10.2.1 allows a purchaser who orders cut lengths and intends to sample after delivery to request extra material on the purchase order, of adequate size to provide test coupons. Clause 11.2 states that if any specimen fails a test, the material it represents may be retested where there is valid reason to believe the result is not representative, and the material may also be re-annealed and retested. Strip is covered by clause 9.2, which refers to B906 except as given in Tables 5 – 7, and plate by clause 9.3, which refers to B906 in full. Tension test specimens are full thickness: the E8/E8M sheet-type specimen under 12.7 mm and the plate-type specimen from 12.7 mm.
How to calculate the weight of N08028 plate
Plate weight is calculated from the dimensions and the density. Using 8.0 g/cm³ (ASTM B709 Table 4 factor of 0.0008 kg/cm²·mm; Euro Inox gives 8.0 g/cm³ for EN 1.4563), one square metre of N08028 plate 1 mm thick weighs 8.0 kg, so the mass of a plate is density × thickness (mm) × width (m) × length (m).
| Example | Calculation | Theoretical mass |
|---|---|---|
| N08028 plate 10 × 2 000 × 6 000 mm | 8.0 × 10 × 2.0 × 6.0 | about 960 kg |
| N08028 sheet 3 × 1 219 × 2 438 mm | 8.0 × 3 × 1.219 × 2.438 | about 71.3 kg |
Actual weight differs from theoretical weight because of thickness tolerance; whether the invoice uses theoretical or actual weight should be agreed at the order. SHH STEEL shows both on the packing list.
Why choose SHH STEEL for N08028
As an experienced N08028 supplier, we find that buyers usually worry less about price than about getting the right material on time. The table below lists the concerns we hear most often and how SHH STEEL deals with each one.
| Buyer concern | Risk | How SHH STEEL handles it |
|---|---|---|
| Wrong alloy | 904L or another lower-alloyed grade is offered as equivalent. | UNS number and full chemistry are checked on the certificate and by PMI. |
| Availability | Few mills roll N08028 plate. | Mill capability and lead time are confirmed before quotation. |
| Trade name confusion | A branded product is quoted when only the UNS grade is required. | Orders name ASTM B709 and N08028; a brand is supplied only when asked. |
| Minimum order | Mills set high minimums for less common grades. | Orders are consolidated so smaller lots can join a mill rolling where the mill makes the grade. |
| Delivery tracking | Delays at rolling, heat treatment or testing are found too late. | A dedicated person follows the schedule and reports progress at each stage. |
SHH STEEL also offers steel cutting services, bending and forming services, a third-party testing service with partner laboratories, and a worldwide shipping service. See our full range of stainless steel sheets and plates.
FAQ
-
What is N08028 equivalent to?
- UNS N08028 (Alloy 28) corresponds to EN 1.4563 (X1NiCrMoCu31-27-4) in EN 10088-2. ASTM B709 and EN 10088-2 limits are close but should be checked for dual certification; EN 10088-2 is tighter for carbon, silicon, manganese, sulphur and nickel, so a heat made to 1.4563 usually also meets B709. 904L (N08904) is sometimes offered as an alternative, but it has lower nickel and chromium and is not equivalent. SHH STEEL compares the limits for each order and supplies N08028 or 1.4563 with the matching certificate. Where a project names more than one standard, SHH STEEL lists every applicable limit on the quotation so that the buyer can approve the material before production starts. Purchase orders should name ASTM B709, its edition, the grade, the thickness and the inspection document required, so the certificate can be checked against the same tables.
-
What is the chemical composition of N08028?
- ASTM B709 sets the following limits for N08028, in percent: Carbon (C) ≤ 0.030; Silicon (Si) ≤ 1.00; Manganese (Mn) ≤ 2.50; Phosphorus (P) ≤ 0.030; Sulphur (S) ≤ 0.030; Nickel (Ni) 30.0 – 34.0; Chromium (Cr) 26.0 – 28.0; Molybdenum (Mo) 3.0 – 4.0; Copper (Cu) 0.6 – 1.4; Iron (Fe) Balance. Iron makes up the balance. SHH STEEL checks every certificate against these limits before shipment and can arrange an independent check analysis by a partner laboratory. Product (check) analysis tolerances follow ASTM B906 when a check analysis is ordered. Where a project specification adds requirements beyond ASTM B709, they should be written into the enquiry so the mill can confirm them before rolling. If a drawing names more than one standard, the material must meet each of them, and the certificate should state every standard it claims.
-
What are the mechanical properties of N08028 plate?
- ASTM B709 requires N08028 in the solution-annealed condition to have a tensile strength of at least 500 MPa, a 0.2 % yield strength of at least 214 MPa and an elongation of at least 40 % in 50 mm. A hardness of 70 – 90 HRB is given for information only. These values reflect a fully austenitic alloy with good ductility for forming and welding. SHH STEEL checks the tensile results on the 3.1 certificate for every heat and can arrange third-party witness testing. Test frequency and specimen location follow ASTM B906, and results are reported for each heat and heat-treatment lot. The figures quoted are the limits of ASTM B709; the actual values for a given heat are those reported on the mill test certificate.
-
How is N08028 supplied and heat treated?
- ASTM B709 covers N08028 plate, sheet and strip in the solution-annealed condition; Note 1 recommends heating to at least 1 080 °C and cooling rapidly, and minor cold work such as flattening may follow. General requirements are in ASTM B906. The low carbon content (0.030 % maximum) means welded parts are not normally solution annealed again for corrosion reasons, but this depends on the fabricator's procedure and the service. SHH STEEL supplies solution-annealed material and asks the mill to record the annealing temperature on the certificate, so the fabricator knows the starting condition of every plate. Any post-fabrication heat treatment should be agreed between the purchaser and the fabricator before work starts. Any supplementary test, such as a product analysis or a corrosion test, has to be agreed at the enquiry stage because it cannot be added after delivery.
-
What sizes of N08028 can SHH STEEL supply?
- ASTM B709 covers plate, sheet and strip of N08028; the size range depends on the producing mill. Dimensional and flatness tolerances follow ASTM B906 unless the order specifies tighter values. SHH STEEL confirms with the mill which thicknesses and widths it can roll in N08028, then offers full plates, cut-to-size blanks or slit strip, with cutting and testing services available. Typical N08028 plate orders range from single cut pieces to full mill lots. Lead time is normally 30 – 40 days after order confirmation, depending on size and the mill rolling schedule. Any supplementary test, such as a product analysis or a corrosion test, has to be agreed at the enquiry stage because it cannot be added after delivery. Purchase orders should name ASTM B709, its edition, the grade, the thickness and the inspection document required, so the certificate can be checked against the same tables.
-
Is N08028 a stainless steel or a nickel alloy?
- N08028 sits between the two. With 30.0 – 34.0 % nickel and iron as the balance, it is classified in the UNS N08xxx series of iron-nickel alloys and is covered by ASTM B709 rather than ASTM A240. In Europe, however, the same alloy type is listed as stainless steel 1.4563 in EN 10088-2. For purchasing, the important point is to name the right standard and UNS number. SHH STEEL supplies N08028 to ASTM B709 or ASME SB-709 and 1.4563 to EN 10088-2. SHH STEEL can also supply technical data from the producing mill on request. If a drawing names more than one standard, the material must meet each of them, and the certificate should state every standard it claims. Where a project specification adds requirements beyond ASTM B709, they should be written into the enquiry so the mill can confirm them before rolling.
Conclusion
ASTM B709 UNS N08028 (Alloy 28) Plate is a high-nickel, high-chromium iron-based alloy with molybdenum and copper, the ASTM counterpart of EN 1.4563, for acid and chloride service. SHH STEEL supplies it with full ASTM B709 compliance, 3.1 inspection certificates and optional third-party testing, with a normal lead time of 30 – 40 days. Contact SHH STEEL for availability, sizes and a quotation for your N08028 requirement.