GB/T 713.7 022Cr21Ni3Mo2N (S22153) is a lean duplex stainless steel plate for pressure equipment, equivalent in family to ASTM A240 S32003. Under GB/T 713.7-2023 it is delivered solution treated with Rp0.2 ≥485 / 450 MPa and Rm ≥ 690 / 655 MPa (Table 17). SHH STEEL supplies it in 0.30 – 100 mm, cut to size, with heat and product analysis on EN 10204 3.1 or 3.2 certificates.
Keywords
GB/T 713.7 S22153, 022Cr21Ni3Mo2N S22153, 022Cr21Ni3Mo2N pressure vessel plate, GB/T 713.7-2023 stainless plate, S22153 vs S32003, GB/T 24511 S22153, S22153 chemical composition, pressure equipment stainless steel plate, ASTM A240 S32003 equivalent, S22153 mechanical properties, duplex stainless steel plate, S32003 PREN
Equivalent Grades:
ASTM A240 UNS S32003 — Material Specification: GB/T 713.7-2023 (022Cr21Ni3Mo2N, unified code S22153; replaces GB/T 24511-2017) — Delivery: solution treated (regime per Annex C), water quench or other rapid cooling
Share:
Overview
Specification
Chemical Composition
Product Analysis
Mechanical Properties
Heat Treatment
Phase Balance & Temperature Limits
Equivalent Grades
Welding & Fabrication
Corrosion Resistance
Applications
Grade Comparison
Dimensions
Surface & Processing
Testing & Certificates
Ordering
Mill Sourcing
FAQ
Conclusion

GB/T 713.7 022Cr21Ni3Mo2N: what it is and who uses it

022Cr21Ni3Mo2N S22153 is listed in GB/T 713.7-2023, the Chinese standard for pressure equipment stainless steel plate, as a lean duplex grade that saves nickel and molybdenum while doubling austenitic proof strength. As a GB/T 713.7-2023 stainless plate it is ordered by vessel and heat-exchanger shops that design to GB/T 150 and the TSG 21 safety rules, and by EPC contractors who must deliver Chinese-code equipment abroad. Its ASTM A240 S32003 equivalent is the nearest foreign grade by chemistry.

Reading the designation: the leading digits give the carbon level (≤ 0.030%); the element symbols that follow give the approximate contents of the main alloying elements in percent. S22153 is the unified numeric code (ISC). The grade was previously certified as GB/T 24511 S22153 until GB/T 24511-2017 was withdrawn on 1 March 2024; most chemistries carried over, but the 2023 edition revised some austenitic strength values and added impact data, so old certificates should be checked against the new tables. Every 022Cr21Ni3Mo2N pressure vessel plate is tested and certified to the 2023 edition.

SHH STEEL produces and exports stainless plate from Shanghai, works as a sales agent for mills including TISCO, Baosteel and POSCO, and runs its own processing warehouse for cutting and polishing. 022Cr21Ni3Mo2N is part of our GB/T 713.7-2023 pressure vessel stainless plate range; for the general-purpose version of the same grade see GB/T 4237 022Cr21Ni3Mo2N S22153.

Why designers specify S22153

Material selection for a Chinese-code pressure vessel starts with the design conditions: medium, temperature, pressure and the minimum design metal temperature. Duplex grades are chosen when a designer needs about twice the proof strength of an austenitic grade together with resistance to chloride stress-corrosion cracking, which allows thinner walls and lighter vessels. GB/T 150 lists the permitted plate standards and allowable stresses, and the material must be supplied with a certificate that ties every plate to its heat. Because 022Cr21Ni3Mo2N is listed in GB/T 713.7-2023, it can be used directly under GB/T 150 without a separate material evaluation, which saves time on approvals compared with a foreign grade.

Who buys it

Our customers for this grade include pressure vessel fabricators in China and Southeast Asia, EPC contractors building Chinese-designed plants in the Middle East, Africa and Central Asia, and maintenance teams that need like-for-like replacement plate for equipment originally built to GB/T 24511 or GB/T 713.7. Export buyers often need the plate certified to GB/T 713.7 and checked against an ASTM or EN grade at the same time, which we arrange with the mill before rolling.

What the standard covers for this grade

Item GB/T 713.7-2023 requirement / SHH STEEL supply
Standard GB/T 713.7-2023 (in force since 1 March 2024; replaces GB/T 24511-2017)
Grade / unified code 022Cr21Ni3Mo2N / S22153
Steel class Austenitic-ferritic (duplex)
Chemical composition Table 14 (heat analysis); product analysis deviations per GB/T 713.1
Mechanical properties Table 17: Rp0.2 ≥ 485 / 450 MPa, Rm ≥ 690 / 655 MPa, A ≥ 25%
Product forms Hot-rolled thick plate, hot-rolled plate and strip, cold-rolled plate and strip, width ≥ 600 mm
Thickness (Table 1) 0.30 – 8.00 mm cold rolled; 2.00 – 14.0 mm hot-rolled strip; 6.00 – 100 mm hot-rolled thick plate
Delivery condition Solution treated (Annex C gives the regime)
Edge / accuracy EC trimmed or EM untrimmed; PT.A or PT.B thickness accuracy
Density about 7.8 (Annex A)
Certificate EN 10204 3.1; 3.2 with third-party witness on request

The table is a summary; the purchase order should cite the full standard and edition. Clause 4.2 of GB/T 713.7 requires the surface finish to be named on the order, and the edge and thickness-accuracy codes decide the tolerance class used for acceptance. For coil-cut plate, flatness and camber follow the general rules of GB/T 713.1, which every part of GB/T 713 refers to.

Heat and product analysis limits for 022Cr21Ni3Mo2N

The S22153 chemical composition is the heat (melting) analysis the mill reports for each heat, and it must meet GB/T 713.7-2023 Table 14 in weight percent.

Element 022Cr21Ni3Mo2N heat analysis, % (Table 14) Why it matters
C ≤ 0.030 Strength, weldability and sensitization risk
Si ≤ 1.00 Deoxidation; in heat-resisting grades, oxidation resistance
Mn ≤ 2.00 Austenite stability and hot workability
P ≤ 0.030 Kept low for weld soundness
S ≤ 0.015 Kept low for toughness and weld cracking resistance
Cr 19.50 – 22.50 Passive film and oxidation resistance
Ni 3.00 – 4.00 Austenite stability and toughness
Mo 1.50 – 2.00 Pitting and crevice resistance
N 0.14 – 0.20 Strength and pitting resistance

The product analysis is a check on the finished plate. Clause 7.2.2 of GB/T 713.7 refers to GB/T 713.1 for the permitted deviations; the values below are the customary GB/T 222 / ASTM A480 deviations applied to 022Cr21Ni3Mo2N and should be confirmed against the edition cited in the contract.

Element Heat analysis limit (%) Permitted deviation Product analysis limit (%)
C ≤ 0.030 +0.005 ≤ 0.035
Si ≤ 1.00 +0.05 ≤ 1.05
Mn ≤ 2.00 +0.04 ≤ 2.04
P ≤ 0.030 +0.005 ≤ 0.035
S ≤ 0.015 +0.005 ≤ 0.020
Cr 19.50 – 22.50 −0.2 / +0.25 19.30 – 22.75
Ni 3.00 – 4.00 −0.07 / +0.07 2.93 – 4.07
Mo 1.50 – 2.00 −0.05 / +0.05 1.45 – 2.05
N 0.14 – 0.20 −0.01 / +0.02 0.130 – 0.220

PREN (Cr + 3.3Mo + 16N) calculated from the minimum chemistry is 26.7. Notes to the table state that compositions were adjusted compared with GB/T 3280 and GB/T 4237, so a general-purpose certificate does not automatically meet GB/T 713.7.

Product (check) analysis and PMI

Product (check) analysis is the chemistry measured on a sample taken from the finished plate rather than from the ladle, and it is how a buyer proves the plate matches the certificate.

Under GB/T 713.7 the mill reports the heat analysis as standard. A product analysis is made when the purchase order calls for it, and the result is judged against the heat limits widened by the permitted deviations shown above. Deviations apply to one side of a range only; a heat may not exceed both the lower and upper limit of the same element. Elements marked ‘by agreement’ have no tabulated deviation and should be settled in the contract.

SHH STEEL runs positive material identification (PMI) on every plate in our Shanghai warehouse before it ships. PMI by handheld XRF confirms Cr, Ni, Mo and other alloying elements; it cannot measure carbon or nitrogen, so when low carbon matters we arrange laboratory spark-OES or combustion analysis through our steel testing service. Product analysis results are added to the 3.1 certificate or reported by the third-party inspector on a 3.2 certificate.

Sampling and acceptance

Samples for product analysis are taken across the thickness or from millings so that the result represents the whole plate, not only the surface. If a product analysis falls outside the permitted range, the usual practice under GB/T 713.1 is to retest on additional samples before the plate or batch is rejected. We keep retained samples from tested heats for a period agreed with the customer, which helps when questions arise during fabrication or inspection.

Mechanical properties of 022Cr21Ni3Mo2N plate

The S22153 mechanical properties are the room-temperature values that GB/T 713.7-2023 Table 17 sets for solution treated plate.

Property GB/T 713.7 S22153 (Table 17)
Rp0.2, MPa ≥ 485 / 450
Rm, MPa ≥ 690 / 655
A, % ≥ 25
Hardness HBW ≤ 293, HRC 31 max

Elongation for thickness ≤ 3.00 mm is measured on A50 mm specimens per GB/T 228.1 P5. Where two values are shown, the first applies to thickness ≤ 5.0 mm and the second to thickness > 5.0 mm, which matters for wall-thickness calculations. Design stresses are not taken from this table directly: the vessel designer uses the allowable-stress tables of GB/T 150.2, which are derived from these minimums and from the elevated-temperature data in Annex D where given.

Compared with ASTM A240 S32003, GB/T 713.7 sets its own strength and elongation minimums; a heat can often be dual-certified, but each certificate must state the values tested against each standard.

How designers use these values

The room-temperature minimums are the basis of the allowable stresses in GB/T 150.2. The designer takes the lower of the stress derived from tensile strength and the stress derived from proof strength, applies the code safety factors, and for elevated temperatures uses the temperature-dependent proof strength. For duplex grades the high proof strength usually means the tensile-strength term governs, and the upper temperature limit in the code must be respected. Hardness limits on the certificate are a quick check that the plate has been correctly heat treated: a plate above the maximum hardness has usually been under-treated or cold worked.

Testing frequency

Tensile and hardness tests are made per batch as defined in the inspection rules of GB/T 713.7 clause 9 and GB/T 713.1. A batch is plate from the same heat, the same thickness and the same heat-treatment condition. When the order calls for testing of each plate or each rolled plate, state this explicitly, as it affects cost and lead time.

Annealing / solution treatment

S22153 heat treatment solution treatment is the final heat treatment that sets the structure and properties of the plate, and GB/T 713.7-2023 Annex C gives the recommended regime for 022Cr21Ni3Mo2N. Mills typically solution treat this grade at about 950 – 1 080 °C followed by rapid cooling to keep the austenite/ferrite balance and avoid sigma and chi phases. The actual temperature and cooling method are recorded on the mill certificate.

Clause 7.1.2 allows hot-rolled strip 14.0 – 25.0 mm thick to be levelled and heat treated sheet by sheet. After heavy cold forming or hot forming of heads, the fabricator should follow GB/T 150.4 on whether re-treatment is needed; for duplex plate, any re-treatment must be a full solution treatment; stress relieving in the 300 – 1 000 °C range causes embrittling phases.

What can go wrong

An incorrectly heat-treated plate shows up as high hardness, low elongation or, in corrosion tests, as intergranular attack. Slow cooling or holding in the range of about 700 – 950 °C forms sigma and chi phases that sharply reduce toughness and corrosion resistance, so cooling must be fast. When we receive plate, our engineers check the heat-treatment record on the certificate against Annex C and the hardness result before releasing the material.

Phase balance and service temperature limits

Phase balance is the ratio of austenite to ferrite in 022Cr21Ni3Mo2N, which the mill controls through chemistry and solution treatment to give the grade its strength and stress-corrosion resistance.

Point Guidance
Typical ferrite About 40 – 60% after solution treatment; ferrite measurement by agreement
Upper limit Usually about 250 – 300 °C in pressure codes because of 475 °C embrittlement
Lower limit Set by the design code; impact testing at the minimum design temperature as agreed
Intermetallics Sigma and chi form at about 700 – 950 °C; avoid slow cooling and over-long heating

Confirm both limits against GB/T 150 and the project specification before choosing duplex.

Buyers comparing the S32003 PREN with this grade should use the same formula and the minimum chemistry of each standard, since the ranges differ slightly.

Design checklist for this service

  • Confirm the minimum and maximum design metal temperatures against the limits in GB/T 150 for this material.
  • State on the order every test that the design relies on, because tests that are ‘by agreement’ are not performed unless they are written into the contract.
  • Check that weld procedures, filler metals and any post-weld treatment are qualified for the same temperature range as the base metal.
  • Keep the mill certificate, the inspection report and the weld records together in the vessel data book, as required for registration with the special-equipment authority.

022Cr21Ni3Mo2N equivalent grades: ASTM, EN, former China

A 022Cr21Ni3Mo2N equivalent grade is a grade in another standard with similar chemistry and properties, not an interchangeable certificate.

Standard system Equivalent / closest grade
GB/T 713.7-2023 022Cr21Ni3Mo2N, S22153
GB/T 24511-2017 (superseded) 022Cr21Ni3Mo2N, S22153
ASTM A240 / ASME SA-240 UNS S32003

Equivalence is by alloy family, not certificate. Replacing S22153 with a foreign grade in a Chinese-code vessel needs approval from the designer and, where required, the special-equipment inspection authority; the reverse also applies to ASME or PED equipment built from GB/T plate.

Welding and fabrication of 022Cr21Ni3Mo2N

Welding of 022Cr21Ni3Mo2N is done by GTAW, SMAW, GMAW or SAW with 2209 or 2307-type filler metal. Heat input is typically held in a window of about 0.5 – 2.5 kJ/mm with interpass at or below about 100 – 150 °C, so the weld and HAZ keep a sound phase balance. Pickle and passivate welds for corrosive service.

Weld procedures are qualified to NB/T 47014 for Chinese-code equipment, or to ASME IX for export projects. Cold forming of heads and shells is normal for this grade; duplex plate needs about twice the forming force of austenitic plate and has more springback. Plasma, laser and waterjet cutting are all suitable; remove heat-tinted edges before welding.

Practical welding notes

  • Clean the joint area with stainless-only brushes and solvent; carbon steel contamination causes rust spots.
  • Use argon with a small nitrogen addition for root and shielding gas to keep the weld austenite level.
  • Avoid autogenous welds without filler, as they give too much ferrite.
  • Do not stress relieve; any heat treatment must be a full solution treatment.

Our warehouse can supply bevelled edges and cut blanks ready for welding, which reduces work in the fabrication shop.

Corrosion resistance and PREN of 022Cr21Ni3Mo2N

Corrosion resistance of 022Cr21Ni3Mo2N is set by its chromium, molybdenum and nitrogen content: it offers corrosion resistance around the 304 – 316 range with much higher strength. Its minimum PREN is 26.7.

For welded parts in sensitizing media, an intergranular corrosion test to GB/T 4334 can be ordered. Hydrotest water chloride content should be controlled as required by GB/T 150.4.

Media guide

Medium Typical suitability
Chloride cooling water Good; strong SCC resistance
Seawater Limited, depends on temperature
Organic acids Good
Sour service Per project specification

The table is general guidance. Final material selection should be based on the actual medium, temperature and concentration, and where possible on plant experience or corrosion testing.

Where this plate goes

Applications of 022Cr21Ni3Mo2N follow from its strength and corrosion behaviour as a pressure equipment stainless steel plate. Typical uses:

  • Storage tanks and process vessels replacing 304/316
  • Water treatment and desalination
  • Structural pressure parts where strength saves weight

Buyers specifying 022Cr21Ni3Mo2N for these jobs often compare it with GB/T 713.7 03Cr22Mn5Ni2MoCuN S22294 and GB/T 713.7 022Cr23Ni4MoCuN S23043; the comparison table on this page shows the differences.

Other GB/T 713.7 grades buyers request alongside it: GB/T 713.7 022Cr23Ni5Mo3N S22053.

Selection guidance by application

For storage tanks and low-pressure vessels the decision is usually driven by corrosion resistance and cost, and the plate thickness is moderate. For high-pressure or large-diameter vessels, strength becomes important and duplex plate often allows a thinner wall than austenitic plate, which reduces weight, welding time and cost. For heat exchangers the tube sheets, shells and channels often use different grades, and we can supply all of them in one order with consistent certification.

Choosing between 022Cr21Ni3Mo2N and its neighbours

On S22153 vs S32003, the alloy family is the same, but GB/T 713.7 sets its own chemistry limits and strength minimums. The table compares the grades buyers most often weigh it against, using GB/T 713.7-2023 values.

Grade Key chemistry, % Rp0.2 min, MPa Rm, MPa
GB/T 713.7 S22153 C ≤ 0.030, Cr 19.50 – 22.50, Ni 3.00 – 4.00, Mo 1.50 – 2.00, N 0.14 – 0.20 485 / 450 ≥ 690 / 655
GB/T 713.7 03Cr22Mn5Ni2MoCuN S22294 C ≤ 0.040, Cr 21.00 – 22.00, Ni 1.35 – 1.70, Mo 0.10 – 0.80, N 0.20 – 0.25 530 / 450 ≥ 700 / 650
GB/T 713.7 022Cr23Ni4MoCuN S23043 C ≤ 0.030, Cr 21.50 – 24.50, Ni 3.00 – 5.50, Mo 0.05 – 0.60, N 0.05 – 0.20 400 ≥ 600
GB/T 713.7 022Cr23Ni5Mo3N S22053 C ≤ 0.030, Cr 22.00 – 23.00, Ni 4.50 – 6.50, Mo 3.00 – 3.50, N 0.14 – 0.20 450 ≥ 620

How to choose

Start from the corrosion requirement and the design temperature, then compare strength, availability and cost. A higher-alloy grade is only worth its price when the medium or temperature needs it; a lower-alloy grade that is readily available often gives a shorter lead time. Lean duplex grades replace 304/316 on cost, standard duplex covers most chloride duties, and super duplex is reserved for seawater and hot chlorides. Our engineers can review your design conditions and suggest the most economical grade that meets the code.

Dimensions and plate weight

Dimension Typical supply
Thickness 0.30 – 8.00 mm cold rolled; 2.00 – 14.0 mm hot-rolled strip; 6.00 – 100 mm hot-rolled thick plate
Width 600 – 2 100 mm strip; up to 4 800 mm thick plate
Length Cut to length or coil
Tolerances GB/T 708 / GB/T 709, PT.A or PT.B
Weight thickness (mm) × density (g/cm³) = kg/m²; density about 7.8 (Annex A)

Weight example: a 10 mm plate at 7.9 – 8.0 g/cm³ weighs about 79 – 80 kg/m². Ask for cut-to-size blanks to reduce scrap on heads and shells.

Tolerance and flatness notes

PT.A is the normal thickness accuracy class; PT.B gives a tighter tolerance and is useful when the designer has little corrosion allowance or when plates are rolled into shells with close fit-up requirements. Flatness depends on thickness and width, and cut-to-length plate from coil is usually flatter than as-rolled thick plate. For heads and dished ends, ask us for circular blanks cut to the developed diameter, which reduces handling and scrap at the fabricator.

Surface finish and processing

Finish Description Availability for this grade
No.1 Hot rolled, heat treated, pickled Hot-rolled plate
2B Cold rolled, heat treated, skin passed Cold-rolled sheet, by mill
2D Cold rolled, heat treated, matt Cold-rolled sheet, by mill
No.4 Mechanically polished On request in our warehouse

We offer steel cutting services and stainless surface finishing services in our Shanghai warehouse.

Choosing a finish

No.1 is the standard finish for hot-rolled pressure vessel plate; it is suitable for shells, heads and parts that will be pickled or machined after fabrication. Cold-rolled 2B is used for thin vessels, liners and parts where a smoother surface helps cleaning. Polished finishes are specified for hygienic vessels in food and pharmaceutical plants, where surface roughness limits are part of the design. Plates can be supplied with PE film protection to prevent scratching during fabrication.

Testing and certification

  • Heat chemical analysis on every heat; product analysis by agreement
  • Tensile test and hardness per Table 17
  • Ferrite content and ASTM A923-type intermetallic test by agreement
  • Intergranular corrosion (GB/T 4334) and UT on request
  • 100% PMI and dimensional check by SHH STEEL
  • EN 10204 3.1 certificate; 3.2 with SGS, BV, TUV or a named inspector

Every test result appears on the certificate with the heat number, so the plate can be traced from mill to finished vessel.

Third-party inspection

For export projects, a 3.2 certificate is often required. In that case an independent inspector witnesses sampling and testing at the mill and countersigns the certificate. We coordinate SGS, BV, TUV, Lloyd’s or a client-named inspector, and we schedule witness points so that inspection does not delay rolling. In our warehouse we check dimensions, flatness, surface condition and marking, and repeat PMI on each plate before packing.

What to put on a 022Cr21Ni3Mo2N purchase order

  • Standard and edition: GB/T 713.7-2023
  • Grade and code: 022Cr21Ni3Mo2N / S22153
  • Thickness, width, length and quantity
  • Edge EC or EM; thickness accuracy PT.A or PT.B
  • Surface finish (clause 4.2)
  • Extra tests: impact temperature, IGC, UT, product analysis
  • Certificate type: EN 10204 3.1 or 3.2

Send the list to SHH STEEL and we return a quotation with mill, lead time and stock options.

Common ordering mistakes

  • Citing GB/T 24511 instead of GB/T 713.7-2023 on new orders.
  • Leaving out the surface finish, which clause 4.2 requires.
  • Not stating impact test temperature when the design needs it.
  • Ordering to GB/T 4237 for pressure parts; GB/T 4237 plate is not certified for pressure equipment.

A short technical review before order placement avoids these problems, and our engineering team does this free of charge.

Mill sourcing and lead time

022Cr21Ni3Mo2N is produced by a smaller number of Chinese mills; we place mill orders through the producers we represent and confirm minimum quantities per thickness. Lead time is typically 30-40 days for mill production (production can be scheduled within 30-40 days), and we confirm the rolling slot with the quotation.

Every plate is traceable to its heat number, and copies of the mill certificates stay on file for repeat orders and audits. Mixed-grade and mixed-standard orders can be consolidated in one shipment.

Packing and export documents

Plates are packed on steel or fumigated wooden pallets with waterproof wrapping, edge protectors and steel straps, and each bundle carries labels with grade, standard, heat number, size and weight. Export documents include the commercial invoice, packing list, mill certificates, certificate of origin and, when required, inspection certificates. We ship from Shanghai port in containers or break bulk, and can consolidate mixed grades in one shipment.

FAQ

What is S22153 stainless steel?
S22153 is the unified numeric code for 022Cr21Ni3Mo2N, a duplex stainless grade listed in GB/T 713.7-2023 for pressure equipment plate. It is supplied solution treated with Rp0.2 ≥485 / 450 MPa and Rm ≥ 690 / 655 MPa per Table 17.
Is S22153 the same as S32003?
S22153 belongs to the same alloy family as ASTM A240 S32003, but the two are not identical specifications. GB/T 713.7 sets its own chemistry limits and strength minimums, so a substitution in a pressure vessel needs approval from the designer.
What is the yield strength of S22153 plate to GB/T 713.7?
Rp0.2 is at least 485 / 450 MPa at room temperature, with Rm ≥ 690 / 655 MPa and A ≥25%, per GB/T 713.7-2023 Table 17. Design allowable stresses are taken from GB/T 150.2, not directly from these minimums.
Is GB/T 24511 still valid?
No. GB/T 24511-2017 was replaced by GB/T 713.7-2023 with effect from 1 March 2024. New orders and designs should cite GB/T 713.7-2023.
What thickness of 022Cr21Ni3Mo2N plate can you supply?
GB/T 713.7 covers 0.30 mm to 100 mm in widths of 600 mm and over. Cold-rolled sheet runs 0.30 – 8.00 mm and hot-rolled thick plate 6.00 – 100 mm; availability by thickness depends on the mill.
What is the PREN of 022Cr21Ni3Mo2N?
The PREN of 022Cr21Ni3Mo2N calculated from minimum chemistry is about 26.7. PREN = Cr + 3.3Mo + 16N is a ranking tool; actual pitting resistance depends on temperature and medium.

Conclusion

GB/T 713.7 022Cr21Ni3Mo2N (S22153) is a duplex pressure-vessel plate grade, known internationally as S32003. It is defined by Table 14 chemistry (C ≤ 0.030, Cr 19.50 – 22.50, Ni 3.00 – 4.00, Mo 1.50 – 2.00, N 0.14 – 0.20) and Table 17 properties of Rp0.2 ≥485 / 450 MPa, Rm ≥ 690 / 655 MPa and A ≥25%. Typical uses include storage tanks and process vessels replacing 304/316, water treatment and desalination and structural pressure parts where strength saves weight.

Before ordering, state the standard edition, the grade name with its code, and any extra tests, so that the mill certificate matches your design documents. SHH STEEL supplies 022Cr21Ni3Mo2N plate from stock and by mill order, cut to size and finished in our own warehouse, with EN 10204 3.1 certificates. For related grades see GB/T 713.7 03Cr22Mn5Ni2MoCuN S22294 and GB/T 713.7 022Cr23Ni4MoCuN S23043, our GB/T 713.7-2023 category and GB/T 4237 022Cr21Ni3Mo2N S22153. Send your sizes and quantities for a quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X