ASTM A106 Grade B Seamless Steel Pipe

ASTM A106/A106M-19 Grade B is seamless carbon steel pipe for high-temperature service, in NPS 1/8 to NPS 48. Grade B requires 60 ksi [415 MPa] minimum tensile strength and 35 ksi [240 MPa] minimum yield, with 0.10 % silicon minimum. The size tables use ASME B36.10-2022 Table 2-1 dimensions and plain-end masses, each checked with the standard formula.
Keywords
ASTM A106 Grade B, A106 seamless pipe, Grade B carbon pipe, high temperature pipe, B36.10 pipe
Equivalent Grades:
Near-equivalents only, not automatic substitutes.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Size Chart
Applications
Equivalent Grades
Sourcing
FAQ
Conclusion

What is ASTM A106 Grade B Seamless Steel Pipe?

ASTM A106/A106M-19 Grade B is seamless carbon steel pipe written for high-temperature service. It is a killed steel: Table 1 requires a silicon minimum of 0.10 %, which is not a requirement of ASTM A53 Grade B. The specified minimum tensile strength is 60 ksi [415 MPa] and the specified minimum yield strength is 35 ksi [240 MPa], not 32 ksi. The product is seamless only; there is no ERW or furnace-welded A106 type.

The scope covers NPS 1/8 to NPS 48 [DN 6 to DN 1200] with nominal (average) wall thickness as given in ASME B36.10M. Other dimensions are permitted if the pipe meets the remaining requirements of A106/A106M. This page uses the 2019 edition extracted for the chemistry and tensile tables. If the order names a later revision, the values on that revision govern.

Material, Manufacture and Scope for ASTM A106 Grade B Seamless Pipe

A106/A106M is the material specification; ASME B36.10 (here the 2022 edition, Table 2-1) supplies the nominal diameters, walls, schedule numbers and plain-end masses. Grade A and Grade C exist in the same standard and must not be inferred from a Grade B enquiry. Heat analysis and product analysis follow A106/A106M, not A53/A53M.

Hydrostatic testing or the alternative nondestructive examination allowed by the specification applies. Pipe NPS 2 [DN 50] and under is subject to a 90° cold-bend test around a mandrel twelve times the B36.10 outside diameter. Flattening and other tests required by A106/A106M are part of the product, not optional extras, unless the specification itself makes them so.

ASTM A106 Grade B Chemical Composition (Heat Analysis)

Table 1 of A106/A106M-19 for Grade B is: carbon 0.30 % maximum, manganese 0.29–1.06 %, phosphorus 0.035 % maximum, sulfur 0.035 % maximum, silicon 0.10 % minimum, and chromium, copper and nickel 0.40 % maximum each, molybdenum 0.15 % maximum and vanadium 0.08 % maximum. Footnote C limits those five residual elements to 1 % combined. Footnote B allows, unless the purchaser specifies otherwise, a 0.06 % manganese increase above the specified maximum for each 0.01 % carbon below the maximum, up to 1.65 % manganese.

The silicon minimum and the 0.035 % phosphorus and sulfur caps are the practical markers that distinguish this analysis from A53 Grade B, which has no silicon minimum and allows 0.05 % phosphorus and 0.045 % sulfur.

Swipe horizontally to view all dimensions.

Element Grade B
Carbon, max 0.30 (see footnote B)
Manganese 0.29–1.06 (see footnote B)
Phosphorus, max 0.035
Sulfur, max 0.035
Silicon, min 0.10
Chromium, max 0.40
Copper, max 0.40
Molybdenum, max 0.15
Nickel, max 0.40
Vanadium, max 0.08
Cr+Cu+Mo+Ni+V 1 % combined

ASTM A106 Grade B Mechanical Properties

Table 2 of A106/A106M-19 requires Grade B to have 60 ksi [415 MPa] minimum tensile strength and 35 ksi [240 MPa] minimum yield strength. The listed basic minimum elongations in 2 in. [50 mm] for Grade B are 30 % longitudinal and 16.5 % transverse for transverse-strip tests and for all small sizes tested in full section, and 22 % longitudinal and 12 % transverse when a standard round 2 in. [50 mm] gauge-length specimen is used. Longitudinal strip-test elongation follows the formula in the standard; transverse strip tests have a stated deduction for thinner walls.

Do not apply the 32 ksi yield that A36 uses for very thick plate, or the 30 ksi Grade A figure, to Grade B pipe.

Swipe horizontally to view all dimensions.

Property Grade B
Tensile strength, min 60 ksi [415 MPa]
Yield strength, min 35 ksi [240 MPa]
Elongation, full-section / transverse-strip basic min, longitudinal 30 %
Elongation, full-section / transverse-strip basic min, transverse 16.5 %
Elongation, standard round 2 in. specimen, longitudinal 22 %
Elongation, standard round 2 in. specimen, transverse 12 %

ASTM A106 Grade B Seamless Pipe Sizes: ASME B36.10-2022 Table 2-1

A106/A106M-19 cites ASME B36.10M for nominal walls in NPS 1/8 to NPS 48. The tables below are formula-checked rows from ASME B36.10-2022 Table 2-1 in that range, including schedule identifications STD, XS and XXS where the table assigns them. Each plain-end mass was recomputed with Wpe = 10.69(D − t)t lb/ft and 0.0246615(D − t)t kg/m; only matching rows are shown. The listing is a dimensional reference, not a mill stock list. Plain-end mass is not threaded-and-coupled mass.

NPS 1/8 through 4 (123 rows).

Swipe horizontally to view all dimensions.

NPS (DN) Schedule / identification Outside diameter, in (mm) Wall thickness, in (mm) Plain-end mass, lb/ft (kg/m)
1/8 (6) 10 0.405 (10.29) 0.049 (1.24) 0.19 (0.28)
1/8 (6) 30 0.405 (10.29) 0.057 (1.45) 0.21 (0.32)
1/8 (6) STD / 40 0.405 (10.29) 0.068 (1.73) 0.24 (0.37)
1/8 (6) XS / 80 0.405 (10.29) 0.095 (2.41) 0.31 (0.47)
1/8 (6) 160 0.405 (10.29) 0.124 (3.15) 0.37 (0.55)
1/8 (6) XXS 0.405 (10.29) 0.19 (4.83) 0.44 (0.65)
1/4 (8) 10 0.54 (13.72) 0.065 (1.65) 0.33 (0.49)
1/4 (8) 30 0.54 (13.72) 0.073 (1.85) 0.36 (0.54)
1/4 (8) STD / 40 0.54 (13.72) 0.088 (2.24) 0.43 (0.63)
1/4 (8) XS / 80 0.54 (13.72) 0.119 (3.02) 0.54 (0.80)
1/4 (8) 160 0.54 (13.72) 0.145 (3.68) 0.61 (0.91)
1/4 (8) XXS 0.54 (13.72) 0.238 (6.05) 0.77 (1.14)
3/8 (10) 10 0.675 (17.14) 0.065 (1.65) 0.42 (0.63)
3/8 (10) 30 0.675 (17.14) 0.073 (1.85) 0.47 (0.70)
3/8 (10) STD / 40 0.675 (17.14) 0.091 (2.31) 0.57 (0.84)
3/8 (10) XS / 80 0.675 (17.14) 0.126 (3.2) 0.74 (1.10)
3/8 (10) 160 0.675 (17.14) 0.158 (4.01) 0.87 (1.30)
3/8 (10) XXS 0.675 (17.14) 0.252 (6.4) 1.14 (1.70)
1/2 (15) 5 0.84 (21.34) 0.065 (1.65) 0.54 (0.80)
1/2 (15) 10 0.84 (21.34) 0.083 (2.11) 0.67 (1.00)
1/2 (15) 30 0.84 (21.34) 0.095 (2.41) 0.76 (1.13)
1/2 (15) STD / 40 0.84 (21.34) 0.109 (2.77) 0.85 (1.27)
1/2 (15) XS / 80 0.84 (21.34) 0.147 (3.73) 1.09 (1.62)
1/2 (15) 160 0.84 (21.34) 0.188 (4.78) 1.31 (1.95)
3/4 (20) 5 1.05 (26.67) 0.065 (1.65) 0.68 (1.02)
3/4 (20) 10 1.05 (26.67) 0.083 (2.11) 0.86 (1.28)
3/4 (20) 30 1.05 (26.67) 0.095 (2.41) 0.97 (1.44)
3/4 (20) STD / 40 1.05 (26.67) 0.113 (2.87) 1.13 (1.68)
3/4 (20) XS / 80 1.05 (26.67) 0.154 (3.91) 1.48 (2.19)
3/4 (20) 160 1.05 (26.67) 0.219 (5.56) 1.95 (2.89)
3/4 (20) XXS 1.05 (26.67) 0.308 (7.82) 2.44 (3.64)
1 (25) 5 1.315 (33.4) 0.065 (1.65) 0.87 (1.29)
1 (25) 10 1.315 (33.4) 0.109 (2.77) 1.41 (2.09)
1 (25) 30 1.315 (33.4) 0.114 (2.9) 1.46 (2.18)
1 (25) STD / 40 1.315 (33.4) 0.133 (3.38) 1.68 (2.50)
1 (25) XS / 80 1.315 (33.4) 0.179 (4.55) 2.17 (3.24)
1 (25) 160 1.315 (33.4) 0.25 (6.35) 2.85 (4.24)
1 (25) XXS 1.315 (33.4) 0.358 (9.09) 3.66 (5.45)
1-1/4 (32) 5 1.66 (42.16) 0.065 (1.65) 1.11 (1.65)
1-1/4 (32) 10 1.66 (42.16) 0.109 (2.77) 1.81 (2.69)
1-1/4 (32) 30 1.66 (42.16) 0.117 (2.97) 1.93 (2.87)
1-1/4 (32) STD / 40 1.66 (42.16) 0.14 (3.56) 2.27 (3.39)
1-1/4 (32) XS / 80 1.66 (42.16) 0.191 (4.85) 3.00 (4.46)
1-1/4 (32) 160 1.66 (42.16) 0.25 (6.35) 3.77 (5.61)
1-1/4 (32) XXS 1.66 (42.16) 0.382 (9.7) 5.22 (7.76)
1-1/2 (40) 5 1.9 (48.26) 0.065 (1.65) 1.28 (1.90)
1-1/2 (40) 10 1.9 (48.26) 0.109 (2.77) 2.09 (3.11)
1-1/2 (40) 30 1.9 (48.26) 0.125 (3.18) 2.37 (3.54)
1-1/2 (40) STD / 40 1.9 (48.26) 0.145 (3.68) 2.72 (4.05)
1-1/2 (40) XS / 80 1.9 (48.26) 0.2 (5.08) 3.63 (5.41)
1-1/2 (40) 160 1.9 (48.26) 0.281 (7.14) 4.86 (7.24)
1-1/2 (40) XXS 1.9 (48.26) 0.4 (10.16) 6.41 (9.55)
2 (50) 5 2.375 (60.32) 0.065 (1.65) 1.61 (2.39)
2 (50) — 2.375 (60.32) 0.083 (2.11) 2.03 (3.03)
2 (50) 10 2.375 (60.32) 0.109 (2.77) 2.64 (3.93)
2 (50) 30 2.375 (60.32) 0.125 (3.18) 3.01 (4.48)
2 (50) — 2.375 (60.32) 0.141 (3.58) 3.37 (5.01)
2 (50) STD / 40 2.375 (60.32) 0.154 (3.91) 3.66 (5.44)
2 (50) — 2.375 (60.32) 0.172 (4.37) 4.05 (6.03)
2 (50) — 2.375 (60.32) 0.188 (4.78) 4.40 (6.55)
2 (50) XS / 80 2.375 (60.32) 0.218 (5.54) 5.03 (7.48)
2 (50) — 2.375 (60.32) 0.25 (6.35) 5.68 (8.45)
2 (50) — 2.375 (60.32) 0.281 (7.14) 6.29 (9.36)
2 (50) 160 2.375 (60.32) 0.344 (8.74) 7.47 (11.12)
2 (50) XXS 2.375 (60.32) 0.436 (11.07) 9.04 (13.45)
2-1/2 (65) 5 2.875 (73.02) 0.083 (2.11) 2.48 (3.69)
2-1/2 (65) — 2.875 (73.02) 0.109 (2.77) 3.22 (4.80)
2-1/2 (65) 10 2.875 (73.02) 0.12 (3.05) 3.53 (5.26)
2-1/2 (65) — 2.875 (73.02) 0.125 (3.18) 3.67 (5.48)
2-1/2 (65) — 2.875 (73.02) 0.141 (3.58) 4.12 (6.13)
2-1/2 (65) — 2.875 (73.02) 0.156 (3.96) 4.53 (6.74)
2-1/2 (65) — 2.875 (73.02) 0.172 (4.37) 4.97 (7.40)
2-1/2 (65) 30 2.875 (73.02) 0.188 (4.78) 5.40 (8.04)
2-1/2 (65) STD / 40 2.875 (73.02) 0.203 (5.16) 5.80 (8.64)
2-1/2 (65) — 2.875 (73.02) 0.216 (5.49) 6.14 (9.14)
2-1/2 (65) — 2.875 (73.02) 0.25 (6.35) 7.02 (10.44)
2-1/2 (65) XS / 80 2.875 (73.02) 0.276 (7.01) 7.67 (11.41)
2-1/2 (65) 160 2.875 (73.02) 0.375 (9.52) 10.02 (14.91)
2-1/2 (65) XXS 2.875 (73.02) 0.552 (14.02) 13.71 (20.40)
3 (80) 5 3.5 (88.9) 0.083 (2.11) 3.03 (4.52)
3 (80) — 3.5 (88.9) 0.109 (2.77) 3.95 (5.88)
3 (80) 10 3.5 (88.9) 0.12 (3.05) 4.34 (6.46)
3 (80) — 3.5 (88.9) 0.125 (3.18) 4.51 (6.72)
3 (80) — 3.5 (88.9) 0.141 (3.58) 5.06 (7.53)
3 (80) — 3.5 (88.9) 0.156 (3.96) 5.58 (8.30)
3 (80) — 3.5 (88.9) 0.172 (4.37) 6.12 (9.11)
3 (80) 30 3.5 (88.9) 0.188 (4.78) 6.66 (9.92)
3 (80) STD / 40 3.5 (88.9) 0.216 (5.49) 7.58 (11.29)
3 (80) — 3.5 (88.9) 0.25 (6.35) 8.69 (12.93)
3 (80) — 3.5 (88.9) 0.281 (7.14) 9.67 (14.40)
3 (80) XS / 80 3.5 (88.9) 0.3 (7.62) 10.26 (15.27)
3 (80) 160 3.5 (88.9) 0.438 (11.13) 14.34 (21.35)
3 (80) XXS 3.5 (88.9) 0.6 (15.24) 18.60 (27.68)
3-1/2 (90) 5 4 (101.6) 0.083 (2.11) 3.48 (5.18)
3-1/2 (90) — 4 (101.6) 0.109 (2.77) 4.53 (6.75)
3-1/2 (90) 10 4 (101.6) 0.12 (3.05) 4.98 (7.41)
3-1/2 (90) — 4 (101.6) 0.125 (3.18) 5.18 (7.72)
3-1/2 (90) — 4 (101.6) 0.141 (3.58) 5.82 (8.65)
3-1/2 (90) — 4 (101.6) 0.156 (3.96) 6.41 (9.54)
3-1/2 (90) — 4 (101.6) 0.172 (4.37) 7.04 (10.48)
3-1/2 (90) 30 4 (101.6) 0.188 (4.78) 7.66 (11.41)
3-1/2 (90) STD / 40 4 (101.6) 0.226 (5.74) 9.12 (13.57)
3-1/2 (90) — 4 (101.6) 0.25 (6.35) 10.02 (14.92)
3-1/2 (90) — 4 (101.6) 0.281 (7.14) 11.17 (16.63)
3-1/2 (90) XS / 80 4 (101.6) 0.318 (8.08) 12.52 (18.64)
4 (100) 5 4.5 (114.3) 0.083 (2.11) 3.92 (5.84)
4 (100) — 4.5 (114.3) 0.109 (2.77) 5.12 (7.62)
4 (100) 10 4.5 (114.3) 0.12 (3.05) 5.62 (8.37)
4 (100) — 4.5 (114.3) 0.125 (3.18) 5.85 (8.71)
4 (100) — 4.5 (114.3) 0.141 (3.58) 6.57 (9.78)
4 (100) — 4.5 (114.3) 0.156 (3.96) 7.24 (10.78)
4 (100) — 4.5 (114.3) 0.172 (4.37) 7.96 (11.85)
4 (100) 30 4.5 (114.3) 0.188 (4.78) 8.67 (12.91)
4 (100) — 4.5 (114.3) 0.203 (5.16) 9.32 (13.89)
4 (100) — 4.5 (114.3) 0.219 (5.56) 10.02 (14.91)
4 (100) STD / 40 4.5 (114.3) 0.237 (6.02) 10.80 (16.08)
4 (100) — 4.5 (114.3) 0.25 (6.35) 11.36 (16.91)
4 (100) — 4.5 (114.3) 0.281 (7.14) 12.67 (18.87)
4 (100) — 4.5 (114.3) 0.312 (7.92) 13.97 (20.78)
4 (100) XS / 80 4.5 (114.3) 0.337 (8.56) 15.00 (22.32)
4 (100) 120 4.5 (114.3) 0.438 (11.13) 19.02 (28.32)
4 (100) 160 4.5 (114.3) 0.531 (13.49) 22.53 (33.54)
4 (100) XXS 4.5 (114.3) 0.674 (17.12) 27.57 (41.03)

NPS 5 through 12 (119 rows).

Swipe horizontally to view all dimensions.

NPS (DN) Schedule / identification Outside diameter, in (mm) Wall thickness, in (mm) Plain-end mass, lb/ft (kg/m)
5 (125) 5 5.563 (141.3) 0.083 (2.11) 4.86 (7.24)
5 (125) 5 5.563 (141.3) 0.109 (2.77) 6.36 (9.46)
5 (125) 5 5.563 (141.3) 0.125 (3.18) 7.27 (10.83)
5 (125) 10 5.563 (141.3) 0.134 (3.4) 7.78 (11.56)
5 (125) 5 5.563 (141.3) 0.156 (3.96) 9.02 (13.41)
5 (125) 5 5.563 (141.3) 0.188 (4.78) 10.80 (16.09)
5 (125) 5 5.563 (141.3) 0.219 (5.56) 12.51 (18.61)
5 (125) STD / 40 5.563 (141.3) 0.258 (6.55) 14.63 (21.77)
5 (125) 5 5.563 (141.3) 0.281 (7.14) 15.87 (23.62)
5 (125) 5 5.563 (141.3) 0.312 (7.92) 17.51 (26.05)
5 (125) 5 5.563 (141.3) 0.344 (8.74) 19.19 (28.57)
5 (125) XS / 80 5.563 (141.3) 0.375 (9.52) 20.80 (30.94)
5 (125) 120 5.563 (141.3) 0.5 (12.7) 27.06 (40.28)
5 (125) 160 5.563 (141.3) 0.625 (15.88) 32.99 (49.12)
5 (125) XXS 5.563 (141.3) 0.75 (19.05) 38.59 (57.43)
6 (150) — 6.625 (168.28) 0.083 (2.11) 5.80 (8.65)
6 (150) 5 6.625 (168.28) 0.109 (2.77) 7.59 (11.31)
6 (150) — 6.625 (168.28) 0.125 (3.18) 8.69 (12.95)
6 (150) 10 6.625 (168.28) 0.134 (3.4) 9.30 (13.83)
6 (150) — 6.625 (168.28) 0.141 (3.58) 9.77 (14.54)
6 (150) — 6.625 (168.28) 0.156 (3.96) 10.79 (16.05)
6 (150) — 6.625 (168.28) 0.172 (4.37) 11.87 (17.66)
6 (150) — 6.625 (168.28) 0.188 (4.78) 12.94 (19.27)
6 (150) — 6.625 (168.28) 0.203 (5.16) 13.94 (20.76)
6 (150) — 6.625 (168.28) 0.219 (5.56) 15.00 (22.31)
6 (150) — 6.625 (168.28) 0.25 (6.35) 17.04 (25.36)
6 (150) STD / 40 6.625 (168.28) 0.28 (7.11) 18.99 (28.26)
6 (150) — 6.625 (168.28) 0.312 (7.92) 21.06 (31.32)
6 (150) — 6.625 (168.28) 0.344 (8.74) 23.10 (34.39)
6 (150) — 6.625 (168.28) 0.375 (9.52) 25.05 (37.27)
6 (150) XS / 80 6.625 (168.28) 0.432 (10.97) 28.60 (42.56)
6 (150) — 6.625 (168.28) 0.5 (12.7) 32.74 (48.73)
6 (150) 120 6.625 (168.28) 0.562 (14.27) 36.43 (54.20)
6 (150) — 6.625 (168.28) 0.625 (15.88) 40.09 (59.68)
6 (150) 160 6.625 (168.28) 0.719 (18.26) 45.39 (67.56)
6 (150) — 6.625 (168.28) 0.75 (19.05) 47.10 (70.11)
6 (150) XXS 6.625 (168.28) 0.864 (21.95) 53.21 (79.21)
6 (150) — 6.625 (168.28) 0.875 (22.22) 53.78 (80.04)
8 (200) 5 8.625 (219.08) 0.109 (2.77) 9.92 (14.78)
8 (200) — 8.625 (219.08) 0.125 (3.18) 11.36 (16.93)
8 (200) 10 8.625 (219.08) 0.148 (3.76) 13.41 (19.97)
8 (200) — 8.625 (219.08) 0.156 (3.96) 14.12 (21.01)
8 (200) — 8.625 (219.08) 0.188 (4.78) 16.96 (25.26)
8 (200) — 8.625 (219.08) 0.203 (5.16) 18.28 (27.22)
8 (200) — 8.625 (219.08) 0.219 (5.56) 19.68 (29.28)
8 (200) 20 8.625 (219.08) 0.25 (6.35) 22.38 (33.31)
8 (200) 30 8.625 (219.08) 0.277 (7.04) 24.72 (36.81)
8 (200) — 8.625 (219.08) 0.312 (7.92) 27.73 (41.24)
8 (200) STD / 40 8.625 (219.08) 0.322 (8.18) 28.58 (42.55)
8 (200) — 8.625 (219.08) 0.344 (8.74) 30.45 (45.34)
8 (200) — 8.625 (219.08) 0.375 (9.52) 33.07 (49.20)
8 (200) 60 8.625 (219.08) 0.406 (10.31) 35.67 (53.08)
8 (200) — 8.625 (219.08) 0.438 (11.13) 38.33 (57.08)
8 (200) XS / 80 8.625 (219.08) 0.5 (12.7) 43.43 (64.64)
8 (200) — 8.625 (219.08) 0.562 (14.27) 48.44 (72.08)
8 (200) 100 8.625 (219.08) 0.594 (15.09) 51.00 (75.91)
8 (200) — 8.625 (219.08) 0.625 (15.88) 53.45 (79.58)
8 (200) 120 8.625 (219.08) 0.719 (18.26) 60.77 (90.43)
8 (200) — 8.625 (219.08) 0.75 (19.05) 63.14 (93.97)
8 (200) 140 8.625 (219.08) 0.812 (20.62) 67.82 (100.92)
8 (200) XXS 8.625 (219.08) 0.875 (22.22) 72.49 (107.88)
8 (200) 160 8.625 (219.08) 0.906 (23.01) 74.76 (111.26)
8 (200) — 8.625 (219.08) 1 (25.4) 81.51 (121.32)
10 (250) 5 10.75 (273) 0.134 (3.4) 15.21 (22.61)
10 (250) 10 10.75 (273) 0.156 (3.96) 17.67 (26.27)
10 (250) 10 10.75 (273) 0.165 (4.19) 18.67 (27.78)
10 (250) 10 10.75 (273) 0.188 (4.78) 21.23 (31.62)
10 (250) 10 10.75 (273) 0.203 (5.16) 22.89 (34.08)
10 (250) 10 10.75 (273) 0.219 (5.56) 24.65 (36.67)
10 (250) 20 10.75 (273) 0.25 (6.35) 28.06 (41.76)
10 (250) 10 10.75 (273) 0.279 (7.09) 31.23 (46.49)
10 (250) 30 10.75 (273) 0.307 (7.8) 34.27 (51.01)
10 (250) 10 10.75 (273) 0.344 (8.74) 38.27 (56.96)
10 (250) STD / 40 10.75 (273) 0.365 (9.27) 40.52 (60.29)
10 (250) 10 10.75 (273) 0.438 (11.13) 48.28 (71.88)
10 (250) XS / 60 10.75 (273) 0.5 (12.7) 54.79 (81.53)
10 (250) 10 10.75 (273) 0.562 (14.27) 61.21 (91.05)
10 (250) 80 10.75 (273) 0.594 (15.09) 64.49 (95.98)
10 (250) 10 10.75 (273) 0.625 (15.88) 67.65 (100.69)
10 (250) 100 10.75 (273) 0.719 (18.26) 77.10 (114.71)
10 (250) 10 10.75 (273) 0.812 (20.62) 86.26 (128.34)
10 (250) 120 10.75 (273) 0.844 (21.44) 89.38 (133.01)
10 (250) 10 10.75 (273) 0.875 (22.22) 92.37 (137.42)
10 (250) 10 10.75 (273) 0.938 (23.83) 98.39 (146.43)
10 (250) XXS / 140 10.75 (273) 1 (25.4) 104.23 (155.10)
10 (250) 160 10.75 (273) 1.125 (28.58) 115.75 (172.27)
10 (250) 10 10.75 (273) 1.25 (31.75) 126.94 (188.90)
10 (250) 10 10.75 (273) 1.375 (34.92) 137.80 (205.03)
10 (250) 10 10.75 (273) 1.438 (36.53) 143.15 (213.03)
12 (300) 5 12.75 (323.8) 0.156 (3.96) 21.00 (31.24)
12 (300) — 12.75 (323.8) 0.172 (4.37) 23.13 (34.43)
12 (300) 10 12.75 (323.8) 0.18 (4.57) 24.19 (35.98)
12 (300) — 12.75 (323.8) 0.188 (4.78) 25.25 (37.61)
12 (300) — 12.75 (323.8) 0.203 (5.16) 27.23 (40.55)
12 (300) — 12.75 (323.8) 0.219 (5.56) 29.34 (43.64)
12 (300) 20 12.75 (323.8) 0.25 (6.35) 33.41 (49.71)
12 (300) — 12.75 (323.8) 0.281 (7.14) 37.46 (55.76)
12 (300) — 12.75 (323.8) 0.312 (7.92) 41.48 (61.70)
12 (300) 30 12.75 (323.8) 0.33 (8.38) 43.81 (65.19)
12 (300) — 12.75 (323.8) 0.344 (8.74) 45.62 (67.91)
12 (300) STD 12.75 (323.8) 0.375 (9.52) 49.61 (73.79)
12 (300) 40 12.75 (323.8) 0.406 (10.31) 53.57 (79.71)
12 (300) — 12.75 (323.8) 0.438 (11.13) 57.65 (85.82)
12 (300) XS 12.75 (323.8) 0.5 (12.7) 65.48 (97.44)
12 (300) 60 12.75 (323.8) 0.562 (14.27) 73.22 (108.93)
12 (300) — 12.75 (323.8) 0.625 (15.88) 81.01 (120.59)
12 (300) 80 12.75 (323.8) 0.688 (17.48) 88.71 (132.05)
12 (300) — 12.75 (323.8) 0.75 (19.05) 96.21 (143.17)
12 (300) — 12.75 (323.8) 0.812 (20.62) 103.63 (154.17)
12 (300) 100 12.75 (323.8) 0.844 (21.44) 107.42 (159.87)
12 (300) — 12.75 (323.8) 0.875 (22.22) 111.08 (165.26)
12 (300) — 12.75 (323.8) 0.938 (23.83) 118.44 (176.29)
12 (300) XXS / 120 12.75 (323.8) 1 (25.4) 125.61 (186.92)
12 (300) — 12.75 (323.8) 1.062 (26.97) 132.69 (197.43)
12 (300) 140 12.75 (323.8) 1.125 (28.58) 139.81 (208.08)
12 (300) — 12.75 (323.8) 1.25 (31.75) 153.67 (228.68)
12 (300) 160 12.75 (323.8) 1.312 (33.32) 160.42 (238.69)
12 (300) — 12.75 (323.8) 1.375 (34.92) 167.20 (248.78)
12 (300) — 12.75 (323.8) 1.5 (38.1) 180.39 (268.44)

NPS 14 through 26 (203 rows).

Swipe horizontally to view all dimensions.

NPS (DN) Schedule / identification Outside diameter, in (mm) Wall thickness, in (mm) Plain-end mass, lb/ft (kg/m)
14 (350) 5 14 (355.6) 0.156 (3.96) 23.09 (34.34)
14 (350) — 14 (355.6) 0.188 (4.78) 27.76 (41.36)
14 (350) — 14 (355.6) 0.203 (5.16) 29.94 (44.59)
14 (350) — 14 (355.6) 0.21 (5.33) 30.96 (46.04)
14 (350) — 14 (355.6) 0.219 (5.56) 32.26 (48.00)
14 (350) 10 14 (355.6) 0.25 (6.35) 36.75 (54.69)
14 (350) — 14 (355.6) 0.281 (7.14) 41.21 (61.36)
14 (350) 20 14 (355.6) 0.312 (7.92) 45.65 (67.91)
14 (350) — 14 (355.6) 0.344 (8.74) 50.22 (74.76)
14 (350) STD / 30 14 (355.6) 0.375 (9.52) 54.62 (81.25)
14 (350) — 14 (355.6) 0.406 (10.31) 59.00 (87.79)
14 (350) 40 14 (355.6) 0.438 (11.13) 63.50 (94.55)
14 (350) — 14 (355.6) 0.469 (11.91) 67.84 (100.95)
14 (350) XS 14 (355.6) 0.5 (12.7) 72.16 (107.40)
14 (350) — 14 (355.6) 0.562 (14.27) 80.73 (120.12)
14 (350) 60 14 (355.6) 0.594 (15.09) 85.13 (126.72)
14 (350) — 14 (355.6) 0.625 (15.88) 89.36 (133.04)
14 (350) — 14 (355.6) 0.688 (17.48) 97.91 (145.76)
14 (350) 80 14 (355.6) 0.75 (19.05) 106.23 (158.11)
14 (350) — 14 (355.6) 0.812 (20.62) 114.48 (170.34)
14 (350) — 14 (355.6) 0.875 (22.22) 122.77 (182.69)
14 (350) 100 14 (355.6) 0.938 (23.83) 130.98 (194.98)
14 (350) — 14 (355.6) 1 (25.4) 138.97 (206.84)
14 (350) — 14 (355.6) 1.062 (26.97) 146.88 (218.58)
14 (350) 120 14 (355.6) 1.094 (27.79) 150.93 (224.66)
14 (350) — 14 (355.6) 1.125 (28.58) 154.84 (230.49)
14 (350) 140 14 (355.6) 1.25 (31.75) 170.37 (253.58)
14 (350) 160 14 (355.6) 1.406 (35.71) 189.29 (281.72)
14 (350) — 14 (355.6) 2 (50.8) 256.56 (381.85)
14 (350) — 14 (355.6) 2.125 (53.98) 269.76 (401.52)
14 (350) — 14 (355.6) 2.2 (55.88) 277.51 (413.04)
14 (350) — 14 (355.6) 2.5 (63.5) 307.34 (457.43)
16 (400) 5 16 (406.4) 0.165 (4.19) 27.93 (41.56)
16 (400) — 16 (406.4) 0.188 (4.78) 31.78 (47.34)
16 (400) — 16 (406.4) 0.203 (5.16) 34.28 (51.06)
16 (400) — 16 (406.4) 0.219 (5.56) 36.95 (54.96)
16 (400) 10 16 (406.4) 0.25 (6.35) 42.09 (62.65)
16 (400) — 16 (406.4) 0.281 (7.14) 47.22 (70.30)
16 (400) 20 16 (406.4) 0.312 (7.92) 52.32 (77.83)
16 (400) — 16 (406.4) 0.344 (8.74) 57.57 (85.71)
16 (400) STD / 30 16 (406.4) 0.375 (9.52) 62.64 (93.18)
16 (400) — 16 (406.4) 0.406 (10.31) 67.68 (100.71)
16 (400) — 16 (406.4) 0.438 (11.13) 72.86 (108.49)
16 (400) — 16 (406.4) 0.469 (11.91) 77.87 (115.87)
16 (400) XS / 40 16 (406.4) 0.5 (12.7) 82.85 (123.31)
16 (400) — 16 (406.4) 0.562 (14.27) 92.75 (138.00)
16 (400) — 16 (406.4) 0.625 (15.88) 102.72 (152.94)
16 (400) 60 16 (406.4) 0.656 (16.66) 107.60 (160.13)
16 (400) — 16 (406.4) 0.688 (17.48) 112.62 (167.66)
16 (400) — 16 (406.4) 0.75 (19.05) 122.27 (181.98)
16 (400) — 16 (406.4) 0.812 (20.62) 131.84 (196.18)
16 (400) 80 16 (406.4) 0.844 (21.44) 136.74 (203.54)
16 (400) — 16 (406.4) 0.875 (22.22) 141.48 (210.52)
16 (400) — 16 (406.4) 0.938 (23.83) 151.03 (224.83)
16 (400) — 16 (406.4) 1 (25.4) 160.35 (238.66)
16 (400) 100 16 (406.4) 1.031 (26.19) 164.98 (245.57)
16 (400) — 16 (406.4) 1.062 (26.97) 169.59 (252.37)
16 (400) — 16 (406.4) 1.125 (28.58) 178.89 (266.30)
16 (400) — 16 (406.4) 1.188 (30.18) 188.11 (280.01)
16 (400) 120 16 (406.4) 1.219 (30.96) 192.61 (286.66)
16 (400) — 16 (406.4) 1.25 (31.75) 197.10 (293.35)
16 (400) 140 16 (406.4) 1.438 (36.53) 223.85 (333.21)
16 (400) 160 16 (406.4) 1.594 (40.49) 245.48 (365.38)
16 (400) — 16 (406.4) 1.75 (44.45) 266.58 (396.77)
18 (450) 5 18 (457.2) 0.165 (4.19) 31.46 (46.81)
18 (450) — 18 (457.2) 0.188 (4.78) 35.80 (53.33)
18 (450) — 18 (457.2) 0.219 (5.56) 41.63 (61.93)
18 (450) 10 18 (457.2) 0.25 (6.35) 47.44 (70.60)
18 (450) — 18 (457.2) 0.281 (7.14) 53.23 (79.25)
18 (450) 20 18 (457.2) 0.312 (7.92) 58.99 (87.75)
18 (450) — 18 (457.2) 0.344 (8.74) 64.93 (96.66)
18 (450) STD 18 (457.2) 0.375 (9.52) 70.65 (105.11)
18 (450) — 18 (457.2) 0.406 (10.31) 76.36 (113.63)
18 (450) 30 18 (457.2) 0.438 (11.13) 82.23 (122.44)
18 (450) — 18 (457.2) 0.469 (11.91) 87.89 (130.79)
18 (450) XS 18 (457.2) 0.5 (12.7) 93.54 (139.22)
18 (450) 40 18 (457.2) 0.562 (14.27) 104.76 (155.88)
18 (450) — 18 (457.2) 0.625 (15.88) 116.09 (172.83)
18 (450) — 18 (457.2) 0.688 (17.48) 127.32 (189.56)
18 (450) 60 18 (457.2) 0.75 (19.05) 138.30 (205.84)
18 (450) — 18 (457.2) 0.812 (20.62) 149.20 (222.01)
18 (450) — 18 (457.2) 0.875 (22.22) 160.18 (238.36)
18 (450) 80 18 (457.2) 0.938 (23.83) 171.08 (254.68)
18 (450) — 18 (457.2) 1 (25.4) 181.73 (270.48)
18 (450) — 18 (457.2) 1.062 (26.97) 192.29 (286.15)
18 (450) — 18 (457.2) 1.125 (28.58) 202.94 (302.10)
18 (450) 100 18 (457.2) 1.156 (29.36) 208.15 (309.78)
18 (450) — 18 (457.2) 1.188 (30.18) 213.51 (317.82)
18 (450) — 18 (457.2) 1.25 (31.75) 223.82 (333.13)
18 (450) 120 18 (457.2) 1.375 (34.92) 244.37 (363.66)
18 (450) 140 18 (457.2) 1.562 (39.67) 274.48 (408.48)
18 (450) 160 18 (457.2) 1.781 (45.24) 308.79 (459.62)
20 (500) 5 20 (508) 0.188 (4.78) 39.82 (59.32)
20 (500) 20 20 (508) 0.219 (5.56) 46.31 (68.89)
20 (500) 10 20 (508) 0.25 (6.35) 52.78 (78.56)
20 (500) 20 20 (508) 0.281 (7.14) 59.23 (88.19)
20 (500) 20 20 (508) 0.312 (7.92) 65.66 (97.68)
20 (500) 20 20 (508) 0.344 (8.74) 72.28 (107.61)
20 (500) STD / 20 20 (508) 0.375 (9.52) 78.67 (117.03)
20 (500) 20 20 (508) 0.406 (10.31) 85.04 (126.54)
20 (500) 20 20 (508) 0.438 (11.13) 91.59 (136.38)
20 (500) 20 20 (508) 0.469 (11.91) 97.92 (145.71)
20 (500) XS / 30 20 (508) 0.5 (12.7) 104.23 (155.13)
20 (500) 20 20 (508) 0.562 (14.27) 116.78 (173.75)
20 (500) 40 20 (508) 0.594 (15.09) 123.23 (183.43)
20 (500) 20 20 (508) 0.625 (15.88) 129.45 (192.73)
20 (500) 20 20 (508) 0.688 (17.48) 142.03 (211.45)
20 (500) 20 20 (508) 0.75 (19.05) 154.34 (229.71)
20 (500) 60 20 (508) 0.812 (20.62) 166.56 (247.84)
20 (500) 20 20 (508) 0.875 (22.22) 178.89 (266.20)
20 (500) 20 20 (508) 0.938 (23.83) 191.14 (284.54)
20 (500) 20 20 (508) 1 (25.4) 203.11 (302.30)
20 (500) 80 20 (508) 1.031 (26.19) 209.06 (311.19)
20 (500) 20 20 (508) 1.062 (26.97) 215.00 (319.94)
20 (500) 20 20 (508) 1.125 (28.58) 227.00 (337.91)
20 (500) 20 20 (508) 1.188 (30.18) 238.91 (355.63)
20 (500) 20 20 (508) 1.25 (31.75) 250.55 (372.90)
20 (500) 100 20 (508) 1.281 (32.54) 256.34 (381.55)
20 (500) 20 20 (508) 1.312 (33.32) 262.10 (390.05)
20 (500) 20 20 (508) 1.375 (34.92) 273.76 (407.41)
20 (500) 120 20 (508) 1.5 (38.1) 296.65 (441.52)
20 (500) 140 20 (508) 1.75 (44.45) 341.41 (508.15)
20 (500) 160 20 (508) 1.969 (50.01) 379.53 (564.85)
22 (550) 5 22 (558.8) 0.188 (4.78) 43.84 (65.31)
22 (550) — 22 (558.8) 0.219 (5.56) 50.99 (75.86)
22 (550) 10 22 (558.8) 0.25 (6.35) 58.13 (86.51)
22 (550) — 22 (558.8) 0.281 (7.14) 65.24 (97.14)
22 (550) — 22 (558.8) 0.312 (7.92) 72.34 (107.60)
22 (550) — 22 (558.8) 0.344 (8.74) 79.64 (118.56)
22 (550) STD / 20 22 (558.8) 0.375 (9.52) 86.69 (128.96)
22 (550) — 22 (558.8) 0.406 (10.31) 93.72 (139.46)
22 (550) — 22 (558.8) 0.438 (11.13) 100.96 (150.33)
22 (550) — 22 (558.8) 0.469 (11.91) 107.95 (160.63)
22 (550) XS / 30 22 (558.8) 0.5 (12.7) 114.92 (171.04)
22 (550) — 22 (558.8) 0.562 (14.27) 128.79 (191.63)
22 (550) — 22 (558.8) 0.625 (15.88) 142.81 (212.62)
22 (550) — 22 (558.8) 0.688 (17.48) 156.74 (233.35)
22 (550) — 22 (558.8) 0.75 (19.05) 170.37 (253.58)
22 (550) — 22 (558.8) 0.812 (20.62) 183.92 (273.68)
22 (550) 60 22 (558.8) 0.875 (22.22) 197.60 (294.03)
22 (550) — 22 (558.8) 0.938 (23.83) 211.19 (314.39)
22 (550) — 22 (558.8) 1 (25.4) 224.49 (334.12)
22 (550) — 22 (558.8) 1.062 (26.97) 237.70 (353.73)
22 (550) 80 22 (558.8) 1.125 (28.58) 251.05 (373.71)
22 (550) — 22 (558.8) 1.188 (30.18) 264.31 (393.44)
22 (550) — 22 (558.8) 1.25 (31.75) 277.27 (412.68)
22 (550) — 22 (558.8) 1.312 (33.32) 290.15 (431.80)
22 (550) 100 22 (558.8) 1.375 (34.92) 303.16 (451.15)
22 (550) — 22 (558.8) 1.438 (36.53) 316.08 (470.50)
22 (550) — 22 (558.8) 1.5 (38.1) 328.72 (489.25)
22 (550) 120 22 (558.8) 1.625 (41.28) 353.94 (526.85)
22 (550) 140 22 (558.8) 1.875 (47.62) 403.38 (600.32)
22 (550) 160 22 (558.8) 2.125 (53.98) 451.49 (672.03)
24 (600) 5 24 (609.6) 0.218 (5.54) 55.42 (82.53)
24 (600) 10 24 (609.6) 0.25 (6.35) 63.47 (94.47)
24 (600) — 24 (609.6) 0.281 (7.14) 71.25 (106.08)
24 (600) — 24 (609.6) 0.312 (7.92) 79.01 (117.52)
24 (600) — 24 (609.6) 0.344 (8.74) 86.99 (129.51)
24 (600) STD / 20 24 (609.6) 0.375 (9.52) 94.71 (140.89)
24 (600) — 24 (609.6) 0.406 (10.31) 102.40 (152.38)
24 (600) — 24 (609.6) 0.438 (11.13) 110.32 (164.27)
24 (600) — 24 (609.6) 0.469 (11.91) 117.98 (175.55)
24 (600) XS 24 (609.6) 0.5 (12.7) 125.61 (186.95)
24 (600) 30 24 (609.6) 0.562 (14.27) 140.81 (209.51)
24 (600) — 24 (609.6) 0.625 (15.88) 156.17 (232.52)
24 (600) 40 24 (609.6) 0.688 (17.48) 171.45 (255.25)
24 (600) — 24 (609.6) 0.75 (19.05) 186.41 (277.44)
24 (600) — 24 (609.6) 0.812 (20.62) 201.28 (299.51)
24 (600) — 24 (609.6) 0.875 (22.22) 216.31 (321.87)
24 (600) — 24 (609.6) 0.938 (23.83) 231.25 (344.25)
24 (600) 60 24 (609.6) 0.969 (24.61) 238.57 (355.04)
24 (600) — 24 (609.6) 1 (25.4) 245.87 (365.94)
24 (600) — 24 (609.6) 1.062 (26.97) 260.41 (387.52)
24 (600) — 24 (609.6) 1.125 (28.58) 275.10 (409.52)
24 (600) — 24 (609.6) 1.188 (30.18) 289.71 (431.25)
24 (600) 80 24 (609.6) 1.219 (30.96) 296.86 (441.80)
24 (600) — 24 (609.6) 1.25 (31.75) 304.00 (452.46)
24 (600) — 24 (609.6) 1.312 (33.32) 318.21 (473.54)
24 (600) — 24 (609.6) 1.375 (34.92) 332.56 (494.90)
24 (600) — 24 (609.6) 1.438 (36.53) 346.83 (516.27)
24 (600) — 24 (609.6) 1.5 (38.1) 360.79 (536.98)
24 (600) 100 24 (609.6) 1.531 (38.89) 367.74 (547.36)
24 (600) — 24 (609.6) 1.562 (39.67) 374.66 (557.57)
24 (600) 120 24 (609.6) 1.812 (46.02) 429.79 (639.62)
24 (600) 140 24 (609.6) 2.062 (52.37) 483.57 (719.68)
24 (600) 160 24 (609.6) 2.344 (59.54) 542.64 (807.68)
26 (650) — 26 (660.4) 0.25 (6.35) 68.82 (102.42)
26 (650) — 26 (660.4) 0.281 (7.14) 77.26 (115.03)
26 (650) 10 26 (660.4) 0.312 (7.92) 85.68 (127.44)
26 (650) — 26 (660.4) 0.344 (8.74) 94.35 (140.46)
26 (650) STD 26 (660.4) 0.375 (9.52) 102.72 (152.81)
26 (650) — 26 (660.4) 0.406 (10.31) 111.08 (165.29)
26 (650) — 26 (660.4) 0.438 (11.13) 119.69 (178.21)
26 (650) — 26 (660.4) 0.469 (11.91) 128.00 (190.47)
26 (650) XS / 20 26 (660.4) 0.5 (12.7) 136.30 (202.86)
26 (650) — 26 (660.4) 0.562 (14.27) 152.83 (227.39)
26 (650) — 26 (660.4) 0.625 (15.88) 169.54 (252.41)
26 (650) — 26 (660.4) 0.688 (17.48) 186.16 (277.15)
26 (650) — 26 (660.4) 0.75 (19.05) 202.44 (301.31)
26 (650) — 26 (660.4) 0.812 (20.62) 218.64 (325.34)
26 (650) — 26 (660.4) 0.875 (22.22) 235.01 (349.71)
26 (650) — 26 (660.4) 0.938 (23.83) 251.30 (374.10)
26 (650) — 26 (660.4) 1 (25.4) 267.25 (397.77)

NPS 28 through 48 (209 rows).

Swipe horizontally to view all dimensions.

NPS (DN) Schedule / identification Outside diameter, in (mm) Wall thickness, in (mm) Plain-end mass, lb/ft (kg/m)
28 (700) — 28 (711.2) 0.25 (6.35) 74.16 (110.38)
28 (700) — 28 (711.2) 0.281 (7.14) 83.26 (123.97)
28 (700) 10 28 (711.2) 0.312 (7.92) 92.35 (137.36)
28 (700) — 28 (711.2) 0.344 (8.74) 101.70 (151.41)
28 (700) STD 28 (711.2) 0.375 (9.52) 110.74 (164.74)
28 (700) — 28 (711.2) 0.406 (10.31) 119.76 (178.21)
28 (700) — 28 (711.2) 0.438 (11.13) 129.05 (192.16)
28 (700) — 28 (711.2) 0.469 (11.91) 138.03 (205.39)
28 (700) XS / 20 28 (711.2) 0.5 (12.7) 146.99 (218.77)
28 (700) — 28 (711.2) 0.562 (14.27) 164.84 (245.26)
28 (700) 30 28 (711.2) 0.625 (15.88) 182.90 (272.30)
28 (700) — 28 (711.2) 0.688 (17.48) 200.87 (299.05)
28 (700) — 28 (711.2) 0.75 (19.05) 218.48 (325.17)
28 (700) — 28 (711.2) 0.812 (20.62) 236.00 (351.17)
28 (700) — 28 (711.2) 0.875 (22.22) 253.72 (377.55)
28 (700) — 28 (711.2) 0.938 (23.83) 271.36 (403.96)
28 (700) — 28 (711.2) 1 (25.4) 288.63 (429.59)
28 (700) — 28 (711.2) 1.062 (26.97) 305.82 (455.10)
30 (750) 5 30 (762) 0.25 (6.35) 79.51 (118.34)
30 (750) — 30 (762) 0.281 (7.14) 89.27 (132.92)
30 (750) 10 30 (762) 0.312 (7.92) 99.02 (147.29)
30 (750) — 30 (762) 0.344 (8.74) 109.06 (162.36)
30 (750) STD 30 (762) 0.375 (9.52) 118.76 (176.67)
30 (750) — 30 (762) 0.406 (10.31) 128.44 (191.12)
30 (750) — 30 (762) 0.438 (11.13) 138.42 (206.10)
30 (750) — 30 (762) 0.469 (11.91) 148.06 (220.32)
30 (750) XS / 20 30 (762) 0.5 (12.7) 157.68 (234.68)
30 (750) — 30 (762) 0.562 (14.27) 176.86 (263.14)
30 (750) 30 30 (762) 0.625 (15.88) 196.26 (292.20)
30 (750) — 30 (762) 0.688 (17.48) 215.58 (320.95)
30 (750) — 30 (762) 0.75 (19.05) 234.51 (349.04)
30 (750) — 30 (762) 0.812 (20.62) 253.36 (377.01)
30 (750) — 30 (762) 0.875 (22.22) 272.43 (405.38)
30 (750) — 30 (762) 0.938 (23.83) 291.41 (433.81)
30 (750) — 30 (762) 1 (25.4) 310.01 (461.41)
30 (750) — 30 (762) 1.062 (26.97) 328.53 (488.88)
30 (750) — 30 (762) 1.125 (28.58) 347.26 (516.93)
30 (750) — 30 (762) 1.188 (30.18) 365.90 (544.68)
30 (750) — 30 (762) 1.25 (31.75) 384.17 (571.79)
32 (800) — 32 (813) 0.25 (6.35) 84.85 (126.32)
32 (800) — 32 (813) 0.281 (7.14) 95.28 (141.90)
32 (800) 10 32 (813) 0.312 (7.92) 105.69 (157.25)
32 (800) — 32 (813) 0.344 (8.74) 116.41 (173.35)
32 (800) STD 32 (813) 0.375 (9.52) 126.78 (188.64)
32 (800) — 32 (813) 0.406 (10.31) 137.12 (204.09)
32 (800) — 32 (813) 0.438 (11.13) 147.78 (220.10)
32 (800) — 32 (813) 0.469 (11.91) 158.08 (235.29)
32 (800) XS / 20 32 (813) 0.5 (12.7) 168.37 (250.65)
32 (800) — 32 (813) 0.562 (14.27) 188.87 (281.09)
32 (800) 30 32 (813) 0.625 (15.88) 209.62 (312.17)
32 (800) 40 32 (813) 0.688 (17.48) 230.29 (342.94)
32 (800) — 32 (813) 0.75 (19.05) 250.55 (373.00)
32 (800) — 32 (813) 0.812 (20.62) 270.72 (402.94)
32 (800) — 32 (813) 0.875 (22.22) 291.14 (433.33)
32 (800) — 32 (813) 0.938 (23.83) 311.47 (463.78)
32 (800) — 32 (813) 1 (25.4) 331.39 (493.35)
32 (800) — 32 (813) 1.062 (26.97) 351.23 (522.80)
32 (800) — 32 (813) 1.125 (28.58) 371.31 (552.88)
32 (800) — 32 (813) 1.188 (30.18) 391.30 (582.64)
32 (800) — 32 (813) 1.25 (31.75) 410.90 (611.72)
34 (850) — 34 (864) 0.25 (6.35) 90.20 (134.31)
34 (850) — 34 (864) 0.281 (7.14) 101.29 (150.88)
34 (850) 10 34 (864) 0.312 (7.92) 112.36 (167.21)
34 (850) — 34 (864) 0.344 (8.74) 123.77 (184.34)
34 (850) STD 34 (864) 0.375 (9.52) 134.79 (200.61)
34 (850) — 34 (864) 0.406 (10.31) 145.80 (217.06)
34 (850) — 34 (864) 0.438 (11.13) 157.14 (234.10)
34 (850) — 34 (864) 0.469 (11.91) 168.11 (250.27)
34 (850) XS / 20 34 (864) 0.5 (12.7) 179.06 (266.63)
34 (850) — 34 (864) 0.562 (14.27) 200.89 (299.04)
34 (850) 30 34 (864) 0.625 (15.88) 222.99 (332.14)
34 (850) 40 34 (864) 0.688 (17.48) 245.00 (364.92)
34 (850) — 34 (864) 0.75 (19.05) 266.58 (396.96)
34 (850) — 34 (864) 0.812 (20.62) 288.08 (428.88)
34 (850) — 34 (864) 0.875 (22.22) 309.84 (461.28)
34 (850) — 34 (864) 0.938 (23.83) 331.52 (493.75)
34 (850) — 34 (864) 1 (25.4) 352.77 (525.30)
34 (850) — 34 (864) 1.062 (26.97) 373.94 (556.73)
34 (850) — 34 (864) 1.125 (28.58) 395.36 (588.83)
34 (850) — 34 (864) 1.188 (30.18) 416.70 (620.60)
34 (850) — 34 (864) 1.25 (31.75) 437.62 (651.65)
36 (900) — 36 (914) 0.25 (6.35) 95.54 (142.14)
36 (900) — 36 (914) 0.281 (7.14) 107.30 (159.68)
36 (900) 10 36 (914) 0.312 (7.92) 119.03 (176.97)
36 (900) — 36 (914) 0.344 (8.74) 131.12 (195.12)
36 (900) STD 36 (914) 0.375 (9.52) 142.81 (212.35)
36 (900) — 36 (914) 0.406 (10.31) 154.48 (229.77)
36 (900) — 36 (914) 0.438 (11.13) 166.51 (247.82)
36 (900) — 36 (914) 0.469 (11.91) 178.14 (264.96)
36 (900) XS / 20 36 (914) 0.5 (12.7) 189.75 (282.29)
36 (900) — 36 (914) 0.562 (14.27) 212.90 (316.63)
36 (900) 30 36 (914) 0.625 (15.88) 236.35 (351.73)
36 (900) — 36 (914) 0.688 (17.48) 259.71 (386.47)
36 (900) 40 36 (914) 0.75 (19.05) 282.62 (420.45)
36 (900) — 36 (914) 0.812 (20.62) 305.44 (454.30)
36 (900) — 36 (914) 0.875 (22.22) 328.55 (488.68)
36 (900) — 36 (914) 0.938 (23.83) 351.57 (523.14)
36 (900) — 36 (914) 1 (25.4) 374.15 (556.62)
36 (900) — 36 (914) 1.062 (26.97) 396.64 (589.98)
36 (900) — 36 (914) 1.125 (28.58) 419.42 (624.07)
36 (900) — 36 (914) 1.188 (30.18) 442.10 (657.81)
36 (900) — 36 (914) 1.25 (31.75) 464.35 (690.80)
38 (950) — 38 (965) 0.312 (7.92) 125.70 (186.94)
38 (950) — 38 (965) 0.344 (8.74) 138.47 (206.11)
38 (950) STD 38 (965) 0.375 (9.52) 150.83 (224.33)
38 (950) — 38 (965) 0.406 (10.31) 163.16 (242.74)
38 (950) — 38 (965) 0.438 (11.13) 175.87 (261.82)
38 (950) — 38 (965) 0.469 (11.91) 188.17 (279.94)
38 (950) XS 38 (965) 0.5 (12.7) 200.44 (298.26)
38 (950) — 38 (965) 0.562 (14.27) 224.92 (334.58)
38 (950) — 38 (965) 0.625 (15.88) 249.71 (371.70)
38 (950) — 38 (965) 0.688 (17.48) 274.42 (408.46)
38 (950) — 38 (965) 0.75 (19.05) 298.65 (444.41)
38 (950) — 38 (965) 0.812 (20.62) 322.80 (480.24)
38 (950) — 38 (965) 0.875 (22.22) 347.26 (516.62)
38 (950) — 38 (965) 0.938 (23.83) 371.63 (553.11)
38 (950) — 38 (965) 1 (25.4) 395.53 (588.57)
38 (950) — 38 (965) 1.062 (26.97) 419.35 (623.90)
38 (950) — 38 (965) 1.125 (28.58) 443.47 (660.01)
38 (950) — 38 (965) 1.188 (30.18) 467.50 (695.77)
38 (950) — 38 (965) 1.25 (31.75) 491.07 (730.74)
40 (1000) 40 40 (1016) 0.312 (7.92) 132.37 (196.90)
40 (1000) 40 40 (1016) 0.344 (8.74) 145.83 (217.11)
40 (1000) STD 40 (1016) 0.375 (9.52) 158.85 (236.30)
40 (1000) 40 40 (1016) 0.406 (10.31) 171.84 (255.71)
40 (1000) 40 40 (1016) 0.438 (11.13) 185.24 (275.82)
40 (1000) 40 40 (1016) 0.469 (11.91) 198.19 (294.92)
40 (1000) XS 40 (1016) 0.5 (12.7) 211.13 (314.23)
40 (1000) 40 40 (1016) 0.562 (14.27) 236.93 (352.53)
40 (1000) 40 40 (1016) 0.625 (15.88) 263.07 (391.67)
40 (1000) 40 40 (1016) 0.688 (17.48) 289.13 (430.45)
40 (1000) 40 40 (1016) 0.75 (19.05) 314.69 (468.37)
40 (1000) 40 40 (1016) 0.812 (20.62) 340.16 (506.17)
40 (1000) 40 40 (1016) 0.875 (22.22) 365.97 (544.57)
40 (1000) 40 40 (1016) 0.938 (23.83) 391.68 (583.08)
40 (1000) 40 40 (1016) 1 (25.4) 416.91 (620.51)
40 (1000) 40 40 (1016) 1.062 (26.97) 442.05 (657.82)
40 (1000) 40 40 (1016) 1.125 (28.58) 467.52 (695.96)
40 (1000) 40 40 (1016) 1.188 (30.18) 492.90 (733.73)
40 (1000) 40 40 (1016) 1.25 (31.75) 517.80 (770.67)
42 (1050) — 42 (1067) 0.344 (8.74) 153.18 (228.10)
42 (1050) STD 42 (1067) 0.375 (9.52) 166.86 (248.27)
42 (1050) — 42 (1067) 0.406 (10.31) 180.52 (268.67)
42 (1050) — 42 (1067) 0.438 (11.13) 194.60 (289.82)
42 (1050) — 42 (1067) 0.469 (11.91) 208.22 (309.90)
42 (1050) XS 42 (1067) 0.5 (12.7) 221.82 (330.21)
42 (1050) — 42 (1067) 0.625 (15.88) 276.44 (411.64)
42 (1050) — 42 (1067) 0.688 (17.48) 303.84 (452.43)
42 (1050) — 42 (1067) 0.75 (19.05) 330.72 (492.33)
42 (1050) — 42 (1067) 0.812 (20.62) 357.52 (532.11)
42 (1050) — 42 (1067) 0.938 (23.83) 411.74 (613.05)
42 (1050) — 42 (1067) 1 (25.4) 438.29 (652.46)
42 (1050) — 42 (1067) 1.062 (26.97) 464.76 (691.75)
42 (1050) — 42 (1067) 1.125 (28.58) 491.57 (731.91)
42 (1050) — 42 (1067) 1.188 (30.18) 518.30 (771.69)
42 (1050) — 42 (1067) 1.25 (31.75) 544.52 (810.60)
44 (1100) — 44 (1118) 0.344 (8.74) 160.54 (239.09)
44 (1100) STD 44 (1118) 0.375 (9.52) 174.88 (260.25)
44 (1100) — 44 (1118) 0.406 (10.31) 189.20 (281.64)
44 (1100) — 44 (1118) 0.438 (11.13) 203.97 (303.82)
44 (1100) — 44 (1118) 0.469 (11.91) 218.25 (324.88)
44 (1100) XS 44 (1118) 0.5 (12.7) 232.51 (346.18)
44 (1100) — 44 (1118) 0.562 (14.27) 260.97 (388.42)
44 (1100) — 44 (1118) 0.625 (15.88) 289.80 (431.62)
44 (1100) — 44 (1118) 0.688 (17.48) 318.55 (474.42)
44 (1100) — 44 (1118) 0.75 (19.05) 346.76 (516.29)
44 (1100) — 44 (1118) 0.812 (20.62) 374.88 (558.04)
44 (1100) — 44 (1118) 0.875 (22.22) 403.38 (600.46)
44 (1100) — 44 (1118) 0.938 (23.83) 431.79 (643.03)
44 (1100) — 44 (1118) 1 (25.4) 459.67 (684.41)
44 (1100) — 44 (1118) 1.125 (28.58) 515.63 (767.85)
44 (1100) — 44 (1118) 1.188 (30.18) 543.70 (809.65)
44 (1100) — 44 (1118) 1.25 (31.75) 571.25 (850.54)
46 (1150) — 46 (1168) 0.344 (8.74) 167.89 (249.87)
46 (1150) STD 46 (1168) 0.375 (9.52) 182.90 (271.99)
46 (1150) — 46 (1168) 0.406 (10.31) 197.88 (294.35)
46 (1150) — 46 (1168) 0.438 (11.13) 213.33 (317.54)
46 (1150) — 46 (1168) 0.469 (11.91) 228.27 (339.56)
46 (1150) XS 46 (1168) 0.5 (12.7) 243.20 (361.84)
46 (1150) — 46 (1168) 0.562 (14.27) 272.98 (406.02)
46 (1150) — 46 (1168) 0.625 (15.88) 303.16 (451.20)
46 (1150) — 46 (1168) 0.688 (17.48) 333.26 (495.97)
46 (1150) — 46 (1168) 0.75 (19.05) 362.79 (539.78)
46 (1150) — 46 (1168) 0.812 (20.62) 392.24 (583.47)
46 (1150) — 46 (1168) 0.875 (22.22) 422.09 (627.86)
46 (1150) — 46 (1168) 0.938 (23.83) 451.85 (672.41)
46 (1150) — 46 (1168) 1 (25.4) 481.05 (715.73)
46 (1150) — 46 (1168) 1.062 (26.97) 510.17 (758.92)
46 (1150) — 46 (1168) 1.125 (28.58) 539.68 (803.09)
46 (1150) — 46 (1168) 1.188 (30.18) 569.10 (846.86)
46 (1150) — 46 (1168) 1.25 (31.75) 597.97 (889.69)
48 (1200) — 48 (1219) 0.344 (8.74) 175.25 (260.86)
48 (1200) STD 48 (1219) 0.375 (9.52) 190.92 (283.96)
48 (1200) — 48 (1219) 0.406 (10.31) 206.56 (307.32)
48 (1200) — 48 (1219) 0.438 (11.13) 222.70 (331.54)
48 (1200) — 48 (1219) 0.469 (11.91) 238.30 (354.54)
48 (1200) XS 48 (1219) 0.5 (12.7) 253.89 (377.81)
48 (1200) — 48 (1219) 0.562 (14.27) 285.00 (423.97)
48 (1200) — 48 (1219) 0.625 (15.88) 316.52 (471.17)
48 (1200) — 48 (1219) 0.688 (17.48) 347.97 (517.95)
48 (1200) — 48 (1219) 0.75 (19.05) 378.83 (563.74)
48 (1200) — 48 (1219) 0.812 (20.62) 409.61 (609.40)
48 (1200) — 48 (1219) 0.875 (22.22) 440.80 (655.81)
48 (1200) — 48 (1219) 0.938 (23.83) 471.90 (702.38)
48 (1200) — 48 (1219) 1 (25.4) 502.43 (747.67)
48 (1200) — 48 (1219) 1.062 (26.97) 532.88 (792.84)
48 (1200) — 48 (1219) 1.125 (28.58) 563.73 (839.04)
48 (1200) — 48 (1219) 1.188 (30.18) 594.50 (884.82)
48 (1200) — 48 (1219) 1.25 (31.75) 624.70 (929.62)

Applications and Service Limits for ASTM A106 Grade B Seamless Pipe

Grade B is the workhorse A106 grade for high-temperature carbon-steel piping, including refinery, process and power lines where the design names A106. It is not a boiler-tube specification by itself, and it is not a structural hollow section. The design temperature, the applicable piping code, and any required impact, sour-service or supplementary tests have to come from the order and the code, not from the grade letter alone.

ASME SA-106 is not assumed on this page. Use the SA designation only when the named BPVC Section II, Part A edition lists SA-106/SA-106M and the identical-with or modified ASTM year can be quoted from that book. An A106 certificate is not an SA-106 certificate.

Near-Equivalents for ASTM A106 Grade B Seamless Pipe: Not Automatic Substitutes

ASTM A53 Grade B Type S is the usual near-comparison: both are seamless 60/35 carbon pipes. They are not interchangeable. A53 has no silicon minimum, allows higher phosphorus and sulfur, stops at NPS 26, and is not written as a high-temperature-service specification. Grade A and Grade C in A106 itself are different strength and carbon levels.

EN 10216-2 P265GH, GB/T 8163, and JIS G 3454 are separate documents. Any substitution is a design decision for the purchaser, not a restamping exercise. SA-106 is held pending a cited Code edition, as noted above.

Sourcing ASTM A106 Grade B Seamless Steel Pipe from SHH STEEL

SHH STEEL reviews enquiries for ASTM A106 Grade B against the A106/A106M edition named on the order, the NPS and specified wall or schedule, the heat-treatment or test supplementary requirements, if any, and the certificate. The B36.10 tables are a checked dimensional reference, not a list of guaranteed mill items. If the purchaser needs SA-106, that Code designation and the Section II year have to be stated; they are not implied by an A106 Grade B description.

ASTM A106 Grade B Seamless Pipe FAQs

Is the yield strength of A106 Grade B 32 ksi or 35 ksi?
35 ksi [240 MPa] minimum, with 60 ksi [415 MPa] minimum tensile strength, per Table 2 of A106/A106M-19. The 32 ksi figure is not the Grade B pipe value.
How does A106 Grade B differ from A53 Grade B seamless?
A106 is a high-temperature-service specification. It requires 0.10 % silicon minimum, caps phosphorus and sulfur at 0.035 %, sets a manganese range, and covers NPS 1/8 to 48. A53 Type S has no silicon minimum and stops at NPS 26.
Which edition is used on this page?
Chemistry and tensile values are taken from ASTM A106/A106M-19. Dimensions and masses are from ASME B36.10-2022 Table 2-1. If the order names a later A106 revision, that revision governs.
Is A106 Grade B the same as SA-106 Grade B?
Not automatically. SA-106 is used only when the named ASME BPVC Section II, Part A edition lists it. An ASTM A106 certificate is not, by itself, an SA-106 certificate.

Conclusion

ASTM A106 Grade B is the seamless, silicon-killed 60 ksi [415 MPa] / 35 ksi [240 MPa] carbon steel pipe of A106/A106M-19 for high-temperature service in NPS 1/8 to 48. It is not A53 Type S and it is not SA-106 unless the Code edition is cited. The size tables are formula-checked ASME B36.10-2022 Table 2-1 rows in that range, used as a dimensional reference. Confirm the edition, grade, wall and any supplementary tests on the order.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X