API 2Y Gr.50 Offshore Steel Plate
API 2Y Gr.50 — offshore platform steel plate overview
API 2Y Gr.50 is quenched-and-tempered offshore structural plate to API Specification 2Y: yield 345–517 MPa [50–75 ksi], tensile 448 MPa [65 ksi] min., Charpy V-notch tested at −40 °C [−40 °F], with low sulphur and a controlled carbon equivalent for heavily welded tubular joints of fixed platforms.
Equivalent grades: EN 10225 S355 grades (no +Q S355 in the 2009 G-list) · EN 10225-1 S355NLO/MLO (nearest by strength) · BS 7191 355EM (nearest designations, plain text — not certificate-equivalent; confirm against the project specification). More grades: Offshore Platform Steel Plates.
The three API plate specifications were written for welded tubular and plate structures of fixed offshore platforms designed to API RP 2A: 2H for normalized carbon–manganese plate used in tubular joints, 2W for TMCP plate and 2Y for quenched-and-tempered plate. All three assume the structure will be welded heavily, inspected for fatigue and loaded through its thickness at nodes, which is why they combine low sulphur, controlled carbon equivalent, Charpy testing at −40 °F and an optional Z-direction test in one product specification.
Offshore steel is bought differently from ship plate or building steel. The structure cannot be docked for repair, it is loaded by waves millions of times over a 25–40 year design life, and its joints are thick, highly restrained and inspected by NDT for fatigue cracks. API 2Y Gr.50 therefore carries three guarantees beyond strength: toughness at low temperature, weldability with a controlled carbon equivalent, and — where ordered — resistance to lamellar tearing through the thickness.
SHH STEEL supplies API 2Y Gr.50 as mill-direct plate with EN 10204 3.1 or 3.2 certification, ultrasonic testing, Z-direction testing and cutting to drawing. The full range is under Offshore Platform Steel Plates.
Where API 2Y Gr.50 sits. API 2Y Gr.50 is the quenched-and-tempered option: it reaches strength through a hardened and tempered microstructure, which keeps properties consistent through heavy sections but needs care in hot forming and post-weld heat treatment. Typical members: jacket legs and braces, tubular joint cans, pile sleeves, launch trusses and topside primary framing on Gulf of Mexico, West Africa and Asia-Pacific platforms.
API 2Y Gr.50: key data at a glance
| Item | API 2Y Gr.50 |
|---|---|
| Standard | API Specification 2H / 2W / 2Y |
| Grade | API 2Y Gr.50 |
| Yield strength, min. | 345–517 MPa [50–75 ksi] |
| Tensile strength | 448 MPa [65 ksi] min. |
| Elongation, min. | 18–22 % (gauge-dependent) (indicative) |
| Charpy V-notch | 34 J [25 ft·lbf] transverse average (typical; supplementary higher values often ordered) |
| Delivery condition | quenched and tempered (QT) |
| Through-thickness | supplementary through-thickness (Z-direction) tensile test, commonly 25–35 % RA ordered |
| Thickness range | up to about 100–150 mm [4–6 in.] depending on spec and mill |
| Certification | EN 10204 3.1 / 3.2; third-party or operator witness on request |
All values are typical of the API Specification 2H / 2W / 2Y grade table and must be checked against the edition named on the purchase order (no local copy of the standard was available for this page — see the note in the ordering section). Yield decreases in steps as thickness increases; for heavy plate the order must state the design thickness so the correct band applies.
API plate specifications are written in inch-pound units with SI conversions; state which governs. Supplementary requirements (S-numbers) — for example Z-direction testing, simulated PWHT, low-sulphur limits or additional Charpy tests — only apply when listed on the order.
API 2Y Gr.50 chemical composition — every alloy element
| Element | Heat (ladle) analysis, % (typical limit) | Product (check) analysis, % | Note |
|---|---|---|---|
| C | 0.16 max. | 0.20 max. (0.16 + 0.04) | |
| Si | 0.05–0.40 | 0.00–0.45 (0.05 − 0.05; 0.40 + 0.05) | |
| Mn | 1.00–1.65 | 0.91–1.77 (1.00 − 0.09; 1.65 + 0.12) | |
| P | 0.030 max. | 0.040 max. (0.030 + 0.010) | low P for toughness and HAZ |
| S | 0.010 max. (0.005 typical by agreement) | 0.020 max. (0.010 + 0.010) | low S for Z-direction ductility |
| Al (total) | 0.015–0.055 | 0.015–0.055 (Al not listed in ASTM A6/A6M Table A – heat limit applies) | grain refiner |
| Nb | 0.04 max. | 0.05 max. (0.04 + 0.01) | microalloy |
| V | 0.08 max. | 0.09 max. (0.08 + 0.01) | microalloy |
| Ti | 0.025 max. | 0.035 max. (0.025 + 0.01) | N-binding |
| Cu | 0.50 max. | 0.53 max. (0.50 + 0.03) | residual / alloy |
| Cr | 0.80 max. | 0.84 max. (0.80 + 0.04) | residual / alloy |
| Ni | 0.50 max. | 0.53 max. (0.50 + 0.03) | toughness |
| Mo | 0.08 max. | 0.09 max. (0.08 + 0.01) | hardenability |
| N | 0.010 max. | 0.015 max. (0.010 + 0.005) | free N harms CTOD |
| Nb+V+Ti | 0.06–0.12 max. (calculated) | not applicable (calculated from heat analysis) | |
| B | 0.005 max. (if added) | not applicable (ASTM A6/A6M Table A, footnote B) | residual unless QT |
| Ca | report if Ca-treated | no numeric heat limit – report actual value | sulphide shape control |
| Ceq (IIW) | 0.40–0.43 max. (calculated; thickness-dependent) | not applicable (calculated from heat analysis) | |
| Pcm | 0.20–0.22 max. (calculated) | not applicable (calculated from heat analysis) | weldability index |
Product (check) analysis column = heat (ladle) limit adjusted by ASTM A6/A6M-19 Table A “Permitted Variations in Product Analysis” (API Spec 2W/2Y plates conform to ASTM A6/A6M, clause 3.1; maximum + “over”, minimum − “under”); arithmetic shown in brackets.
Offshore chemistries are defined more tightly than general structural steel because every element affects either weldability (C, Mn, Cr, Mo, V, Cu, Ni, B through Ceq and Pcm), heat-affected-zone toughness (N, Ti, Nb, Al) or through-thickness ductility (S, Ca, P). For API 2Y Gr.50 the table lists every element the certificate should report; limits shown are indicative values for the API Specification 2H / 2W / 2Y grade family and must be verified against the governing table.
API 2H, 2W and 2Y also allow the purchaser to impose lower sulphur and carbon-equivalent maxima as supplementary requirements; offshore operators routinely do so for joint cans.
Heat vs product analysis: Values above follow peer-consistent tables (hnssteel / katalor / BBN / Regency) for API Spec 2H/2W/2Y style grades. Numeric product limits for C/S/Si/Nb are the highest-confidence peer consensus; other elements are labeled as heat ± product tolerance pending the paid API specification. Mark still subject to verification against the official API Spec.
API 2Y Gr.50 tensile properties by thickness
| Thickness (mm) | Yield ReH min. (MPa) | Tensile Rm (MPa) | Elongation min. |
|---|---|---|---|
| ≤ 16 | 345 | 448 MPa | 18–22 % (gauge-dependent) |
| 16–25 | 345 | 448 MPa | 18–22 % (gauge-dependent) |
| 25–40 | 345 | 448 MPa | 18–22 % (gauge-dependent) |
| 40–63 | 345 | 448 MPa | 18–22 % (gauge-dependent) |
| 63–100 | 335 | 448 MPa | 18–22 % (gauge-dependent) |
Thickness steps are indicative and must be checked: API specifications hold the full yield band to about 2.5 in. and then reduce it. Designers working to ISO 19902, API RP 2A or NORSOK N-004 use the yield of the actual thickness band, so the reduction matters for heavy chords and cans.
Many offshore projects add a maximum yield-to-tensile ratio (often 0.85–0.90, grade-dependent) and an upper yield limit to keep weld metal overmatching. For API 2Y Gr.50 these are project requirements, not always standard requirements, and must be ordered explicitly.
The 355 MPa level is the backbone of offshore construction. Most jacket legs, braces, deck girders and piles are designed at this level because it balances strength, weldability, fatigue performance and availability; fatigue, not static strength, often governs member size, so going higher in strength does not always save weight.
API sets an upper yield limit as well as a minimum, because tubular joint design relies on the brace and chord yielding in a predictable way and on weld metal that overmatches the base plate. An unusually strong plate is therefore not automatically better: it can push the joint outside its design assumptions.
API 2Y Gr.50: Charpy at −40 °C [−40 °F] and delivery condition
API 2Y Gr.50 is delivered quenched and tempered (QT). Impact requirement: 34 J [25 ft·lbf] transverse average (typical; supplementary higher values often ordered). Each value is the mean of three full-size specimens; single values must not fall below the minimum fraction stated in the standard (commonly 70 %).
Quenched-and-tempered plate must not be heated above the tempering temperature during fabrication; PWHT, if required, must stay below it and be simulated on the test coupons.
For heavy plate, offshore projects often require Charpy specimens from mid-thickness as well as near the surface, and testing in the transverse direction. These additions change test cost and lead time, so ask for them in the enquiry for API 2Y Gr.50.
A test temperature of −40 °C [−40 °F] is chosen to sit well below the lowest anticipated service temperature of the structure, giving margin for the strain-ageing, residual stress and constraint present in welded offshore joints. If the project design temperature is lower than usual — Arctic or sub-Arctic fields — the order should specify a lower test temperature or a higher energy, and the mill must confirm it can certify it for API 2Y Gr.50 in the ordered thickness.
API 2Y Gr.50: Z-direction quality and lamellar tearing
Through-thickness status for API 2Y Gr.50: supplementary through-thickness (Z-direction) tensile test, commonly 25–35 % RA ordered. Tubular joints, padeyes, brace-to-chord connections and deck girder flanges carry load perpendicular to the plate surface; plate made from a cast slab has its weakest direction there.
The Z-quality test follows EN 10164 practice (Z15, Z25, Z35 classes by reduction of area) or the equivalent API supplementary requirement; the class must be stated on the order, together with whether testing is per plate or per heat.
For API 2Y Gr.50 the mill test is a tensile specimen machined across the plate thickness with friction-welded extensions; the reduction of area is the acceptance value. Low sulphur, calcium treatment and controlled centreline segregation are the levers that make the value reachable in thick plate. At yield level 50 the stiffeners and brace stubs that land on a chord can pull a plate apart through its thickness if inclusions are elongated — lamellar tearing is a fabrication defect that appears during welding, not in service, so it must be prevented by steel choice.
API 2Y Gr.50: CTOD and low-temperature toughness
CTOD is not a standard requirement for this grade but can be added as an option. In offshore practice CTOD may be required both for steel qualification (per mill and route) and for welding procedure qualification at the node.
Charpy energy at −40 °C [−40 °F] is a quality-control test; CTOD is an engineering test. For API 2Y Gr.50, the designer decides whether CTOD testing of parent plate and weld HAZ is required — typically for nodes, thick-walled joint cans and members where fatigue cracks could grow to a critical size. The project specification sets the test temperature (often −10 °C or the lowest design temperature) and the required CTOD value (0.25 mm is frequently quoted — project-specific, UNCERTAIN).
API 2Y Gr.50 within API Specification 2H / 2W / 2Y
API 2H, 2W and 2Y share a design target — fixed platforms to API RP 2A or ISO 19902 — but differ in metallurgy. Gr.50 is the 50 ksi level used for most jacket steel; Gr.60 is the 60 ksi level used where weight saving matters. Gr.42 also exists in 2H and 2W but is outside this page set.
Operators often overlay their own documents: NORSOK M-120 material data sheets (e.g. MDS for structural plate), NORSOK M-101 for fabrication and M-650 for qualification of manufacturers. Where these apply to API 2Y Gr.50, they add test frequency, chemistry limits and documentation beyond the base standard (MDS numbers not quoted here — confirm with the project).
Supplementary requirements are the real working part of an API plate order. Typical offshore selections include the through-thickness tensile test, low-sulphur and calcium treatment, additional Charpy tests at transverse orientation, simulated post-weld heat treatment of coupons, ultrasonic examination and a cap on carbon equivalent tighter than the base table. A plate certified “API 2W Gr.50” without its S-requirements is a different product from one certified with them, even though both carry the same grade name.
API 2Y Gr.50 against other offshore designations
| Standard | Nearest designation | Remark |
|---|---|---|
| API Specification 2H / 2W / 2Y (this page) | API 2Y Gr.50 | ordered grade |
| EN 10225 | EN 10225 S355 grades (no +Q S355 in the 2009 G-list) | nearest — verify chemistry, impact and Z requirements |
| EN 10225-1 | EN 10225-1 S355NLO/MLO (nearest by strength) | nearest — verify chemistry, impact and Z requirements |
| BS 7191 | BS 7191 355EM | nearest — verify chemistry, impact and Z requirements |
API family: API 2H Gr.50, API 2W Gr.50, API 2W Gr.60, API 2Y Gr.60. Nearest designations are similar in strength and intent but not interchangeable on paper: impact temperature, Z-quality, CTOD scope and chemistry limits differ. A plate can carry two designations only if one heat meets every requirement of both and the certificate names both.
Ship-plate grades such as EH36 are sometimes offered against offshore orders; they meet a similar strength and −40 °C impact level but lack the offshore chemistry limits, Z-testing and CTOD scope, so they are not substitutes for primary offshore structure.
Welding and fabrication of API 2Y Gr.50
Weld API 2Y Gr.50 with low-hydrogen processes (SMAW with basic electrodes, FCAW, SAW) and consumables whose weld-metal Charpy and, where specified, CTOD properties meet the project at −40 °C [−40 °F]. Preheat is calculated from Ceq or Pcm, combined thickness and heat input (EN 1011-2 or AWS D1.1 Annex methods) and recorded in the WPS.
API RP 2A and AWS D1.1 are the usual welding references with API plate; tubular T-, K- and Y-joints need qualified procedures for the specific joint geometry.
For API 2Y Gr.50 the WPS is qualified on plate from the actual supplier and route where possible, covering the heat-input window, preheat, interpass temperature and any PWHT. Offshore projects typically require Charpy tests in weld metal, fusion line and fusion line +2 / +5 mm, plus hardness surveys (often 325 or 350 HV10 max. — project-specific) and, for critical joints, HAZ CTOD.
Quenched-and-tempered plate holds its strength through heavy thickness; cutting edges may need preheat at the higher strengths, and any PWHT must stay below the tempering temperature with simulated-PWHT tests where required.
API 2Y Gr.50: testing, marking and certificates
Mill certificate to EN 10204 3.1 is normal; 3.2 with a third-party or operator witness is common on platform projects, and the operator’s project specification (often based on API RP 2A or ISO 19902) may add requirements such as simulated PWHT or CTOD.
Each plate of API 2Y Gr.50 is marked with the manufacturer, standard, grade, heat and plate number and inspector’s stamp. Receiving inspection should match the stencil to the certificate, check thickness at several points, confirm UT class and Z-test results where ordered, and verify Ceq/Pcm against the WPS range.
API 2Y Gr.50 sizes, stock and lead time
| Thickness (mm) | Width (mm) | Length (mm) | Condition |
|---|---|---|---|
| 10 | 2500 | 6000–12000 | QT |
| 12 | 2500 / 3000 | 6000–12000 | QT |
| 16 | 2500 / 3000 | 6000–12000 | QT |
| 20 | 2500 / 3000 | 6000–12000 | QT |
| 25 | 3000 | 6000–12000 | QT |
| 30 | 3000 | 8000–12000 | QT |
| 40 | 3000 | 8000–12000 | QT |
| 50 | 3000 | 8000–12000 | QT |
| 60 | 2500 / 3000 | 6000–12000 | QT |
| 80 | 2500 | 6000–10000 | QT |
Offshore plate is mostly rolled to order against a project specification; stock covers common thicknesses only. Mill-campaign lead time for API 2Y Gr.50 is typically 6–10 weeks plus testing and freight (commercial estimate).
We cut API 2Y Gr.50 to drawing, bevel, shot-blast and prime, transfer heat numbers to every piece and arrange third-party witness on request.
API plate is frequently rolled for a specific platform project together with its tubular-forming programme; cans are rolled from the plate in a pipe mill or fabrication yard, so the plate order should state forming method and whether simulated forming strain tests are needed.
Mistakes we see on API 2Y Gr.50 orders
- Ordering by strength only (“345 MPa offshore”) without the full designation and route
- Missing Z-quality class for plates loaded through the thickness
- No CTOD or simulated PWHT requirement stated when the project needs it
- Hot forming TMCP or QT plate without checking the mill’s limits
- Accepting ship-plate or general structural grades as substitutes
- Not stating the UT standard and class
For API 2Y Gr.50 the most expensive mistake is late addition of tests — Z, CTOD or simulated PWHT cannot be added once the plates have shipped without re-sampling, and some cannot be done at all.
With API plate the recurring error is ordering the base specification only and assuming the offshore operator’s supplementary requirements are “standard”. They are not: Z-testing, simulated PWHT, extra Charpy sets and tighter carbon equivalent must be listed by number, or the mill will quote and test the base product. A second error is mixing 2H, 2W and 2Y plate in one tubular member without checking that the welding procedure covers each route.
Ordering information for API 2Y Gr.50
Sample line: “Plate, API Specification 2H / 2W / 2Y API 2Y Gr.50, 40 × 3000 × 12000 mm, 20 pcs, Z35, UT EN 10160 S2E3, EN 10204 3.2” — then send it to SHH STEEL.
- Standard and edition: API Specification 2H / 2W / 2Y
- Grade: API 2Y Gr.50
- Thickness, width, length, quantity and tolerance class
- Delivery condition and any limits on fabrication heat treatment
- Impact: temperature (−40 °C [−40 °F]), direction and position; project values if higher
- Through-thickness class (Z25/Z35) and test frequency
- CTOD and simulated PWHT if required
- UT standard and class (EN 10160 / ASTM A578)
- Inspection document (EN 10204 3.1 / 3.2) and witnessing party; NORSOK M-120 MDS if applicable
Note: no local copy of the standard was checked for this page; clause and table numbers are deliberately not quoted, and indicative values must be confirmed against the edition on the order.
FAQ
-
What is API 2Y Gr.50?
- API 2Y Gr.50 is offshore structural plate to API Specification 2H / 2W / 2Y, with minimum yield 345–517 MPa [50–75 ksi] and tensile 448 MPa [65 ksi] min.. API 2Y Gr.50 is the quenched-and-tempered option: it reaches strength through a hardened and tempered microstructure, which keeps properties consistent through heavy sections but needs care in hot forming and post-weld heat treatment. In practice API 2Y Gr.50 is chosen for jacket legs and braces, tubular joint cans, pile sleeves, launch trusses and topside primary framing on Gulf of Mexico, West Africa and Asia-Pacific platforms. The decision usually comes from the design basis: strength level 50, design temperature, joint classification and fatigue category together point to the required grade, and the project material specification then fixes the remaining options. This positioning follows API RP 2A / ISO 19902 design practice; the project material specification can narrow it further. The 355 MPa level is the backbone of offshore construction. Most jacket legs, braces, deck girders and piles are designed at this level because it balances strength, weldability, fatigue performance and availability.
-
What impact toughness does API 2Y Gr.50 guarantee?
- 34 J [25 ft·lbf] transverse average (typical; supplementary higher values often ordered). Impact testing at −40 °C [−40 °F] demonstrates that the plate stays ductile at the lowest service temperatures expected for offshore structures. The Charpy requirement at −40 °C [−40 °F] is the quality-control baseline. Projects may tighten it — a higher average, transverse orientation, testing at the plate quarter-thickness and at mid-thickness for heavy plate — and these must be written into the order before rolling. For API 2Y Gr.50, record the test temperature, specimen orientation and position on the certificate so the operator’s inspector can verify compliance without re-testing.
-
Does API 2Y Gr.50 need through-thickness (Z) testing?
- Supplementary through-thickness (Z-direction) tensile test, commonly 25–35 % RA ordered. Z-testing measures reduction of area across the thickness and is the main protection against lamellar tearing. Lamellar tearing risk rises with plate thickness, joint restraint and weld size. For API 2Y Gr.50 in cruciform or T-joints carrying load through the plate, specify Z-quality and ultrasonic testing of the landing zone; buttering and joint redesign are fabrication-side remedies. Plates for nodes, padeyes and brace landings in API 2Y Gr.50 benefit most from Z-quality; secondary plating rarely needs it.
-
How weldable is API 2Y Gr.50?
- Weldability is governed by Ceq and Pcm, which for 345 MPa-class offshore steel are capped low; delivered quenched and tempered (QT), it is welded with low-hydrogen processes under a qualified procedure. Low carbon equivalent helps, but the qualified procedure decides. For API 2Y Gr.50 we provide the actual heat analysis with Ceq and Pcm values so the welding engineer can check the preheat calculation against the WPS range before production starts. Hardness limits in the HAZ, often required for sour or cathodically protected structures, are checked during procedure qualification of API 2Y Gr.50.
-
What are the nearest equivalents to API 2Y Gr.50?
- Nearest designations: EN 10225 S355 grades (no +Q S355 in the 2009 G-list); EN 10225-1 S355NLO/MLO (nearest by strength); BS 7191 355EM. These are near matches, not certificate equivalents. Substitution between offshore families is a project decision, not a supplier decision: API 2Y Gr.50 can be dual-certified with other offshore grades if one heat meets every requirement of both documents, and the certificate must list both designations. When a project changes standard mid-stream, a written concession listing the replacement grade and any extra tests avoids disputes at final documentation review.
-
Which certificate comes with API 2Y Gr.50?
- EN 10204 3.1 as standard, 3.2 with witness by the purchaser, operator or a classification society on request. The inspector’s stamp and certificate number should be transferred to cut pieces so traceability survives fabrication. Certification is fixed before rolling. Mill certificate to EN 10204 3.1 is normal; 3.2 with a third-party or operator witness is common on platform projects, and the operator’s project specification (often based on API RP 2A or ISO 19902) may add requirements such as simulated PWHT or CTOD. All certificates for API 2Y Gr.50 are issued in English with heat analysis, mechanical results and option results on one document.
-
Is ultrasonic testing included for API 2Y Gr.50?
- UT is an order option for API 2Y Gr.50; offshore projects almost always specify it, usually as a full-body scan plus edge-zone scan, with acceptance class agreed with the engineering contractor before rolling. Ultrasonic testing is normally ordered to EN 10160 (class S2/E3 or better) or ASTM A578 for offshore plate; for API 2Y Gr.50 in node areas the edge zone and the full body are both scanned (class to be stated on the order). UT results for API 2Y Gr.50 are reported plate by plate with the standard and acceptance class named on the certificate.
-
What are sizes, lead times and payment terms?
- Plates 8–150 mm thick, widths to about 3000–4000 mm and lengths to 12–18 m depending on mill. Payment by T/T or L/C at sight; third-party inspection on request. Minimum rolling quantities apply per thickness and grade, and project orders are scheduled into the mill campaign once the specification review is complete. For API 2Y Gr.50 we cut to drawing, bevel and shot-blast in our own workshop, keep heat-number traceability on every piece and pack plate flat with timber spacers for sea freight. Quantities, weights and the document list are confirmed in writing before loading, and the operator’s inspector can witness at the mill or at our yard. Mixed-thickness orders of API 2Y Gr.50 can be consolidated per mill campaign to reduce minimum-quantity surcharges.
Conclusion
API 2Y Gr.50 is a API Specification 2H / 2W / 2Y offshore structural plate: yield 345–517 MPa [50–75 ksi], impact at −40 °C [−40 °F], delivered quenched and tempered (QT). Order it with the full designation, Z-quality, UT and certification stated before rolling.
SHH STEEL supplies API 2Y Gr.50 with EN 10204 certificates, third-party witness, cutting and UT. Send grade, sizes, quantities and project specification for a quotation.