SAE 304 Stainless: ASTM A240 Carbon Limits
SAE 304 Stainless: ASTM A240 Carbon Limits
Description: Carbon limits for SAE 304, 304L and 304H under ASTM A240, with a composition comparison across ASTM, EN, JIS, GB/T and ISO standards.
Keywords: SAE 304 composition; ASTM A240 304 carbon content; 304 vs 304L vs 304H; UNS S30400 S30403 S30409; 1.4301 vs SUS304 vs 06Cr19Ni10; ASTM A312 304L carbon
Introduction
SAE/AISI Type 304 stainless steel (UNS S30400) is the most widely used austenitic chromium–nickel stainless steel. In flat-rolled form (plate, sheet and strip) it is commonly ordered to ASTM A240/A240M, Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications. Closely related low-carbon and high-carbon variants, Type 304L (UNS S30403) and Type 304H (UNS S30409), share the same broad 18Cr–8Ni family but differ principally in carbon content.
Those carbon differences matter for weldability, resistance to intergranular corrosion after thermal exposure, and elevated-temperature strength. Limits are also product-form dependent: the maximum carbon for Type 304 or 304L under ASTM A240 (flat-rolled) is not always identical to pipe or tube specifications such as ASTM A312 or ASTM A213. Older AISI handbook values and some bar standards (for example ASTM A276) likewise retain slightly different figures, and European, Japanese, Chinese and ISO standards each define their own 304-type compositions.
This article summarizes carbon limits commonly associated with Types 304, 304L and 304H under ASTM A240, explains why carbon is controlled, compares the full chemical composition of 304-family grades across major standards, contrasts flat-rolled and tubular rules, and lists typical chromium and nickel ranges. Readers should verify all numerical limits against the current official standard; secondary tables can lag revisions, and unofficial PDF copies are not authoritative.
What SAE/AISI 304 Is, and How It Relates to ASTM A240
Type 304 is an austenitic stainless steel: its room-temperature microstructure is predominantly face-centered cubic austenite, stabilized by nickel in an iron–chromium base. It is not hardenable by quench-and-temper heat treatment; strength is increased by cold work. In the Unified Numbering System it is UNS S30400. Related designations include SAE 304 (SAE 30304), AISI 304, EN 1.4301 (X5CrNi18-10), JIS SUS304 and GB/T 06Cr19Ni10 (S30408). These designations are close equivalents rather than identical specifications; their composition limits differ in detail, as shown below.
ASTM A240/A240M specifies chemistry, mechanical properties, heat-treatment condition and testing for flat-rolled chromium and chromium–nickel stainless steels for pressure vessels and general applications. An “A240 Type 304 plate” order requires Table 1 chemistry and Table 2 tensile values of that specification (adopted as ASME SA-240 for Code work). Bars, shapes, pipe and tube use other ASTM standards that may list different composition envelopes for the same UNS number.
Type 304L (UNS S30403) and Type 304H (UNS S30409) appear in the same A240 chemistry table. They are 304-family variants defined mainly by carbon: “L” for low carbon (reduced sensitization risk in welding) and “H” for controlled higher carbon (creep and high-temperature strength). Dual certification as both 304 and 304L is common when a melt meets 304L’s carbon ceiling and 304’s higher minimum strength.
Why Carbon Content Matters
Carbon in austenitic stainless steel is a double-edged alloying element.
Sensitization and weld-related corrosion. When austenitic grades are held or cooled slowly through roughly 450–850 °C (about 840–1560 °F), including many weld heat-affected zones, carbon can form chromium-rich carbides at grain boundaries. Local chromium depletion can cause intergranular corrosion where unsensitized 304 would otherwise perform adequately. Lowering carbon (304L) lengthens the incubation time for carbide precipitation and improves as-welded corrosion performance in medium and heavy sections without relying solely on post-weld solution annealing.
Weldability. 304L is preferred for welded tanks, process equipment and piping in corrosive service when solution annealing after fabrication is impractical. For thin sheet formed into light fabrications that are not heavily welded, standard 304 is often adequate.
Elevated-temperature strength. Carbon contributes to high-temperature tensile and creep strength. Pressure-vessel and piping codes often require a minimum carbon content (commonly 0.04%) for austenitic grades used above roughly 525–550 °C (about 1000 °F), depending on the code edition. Type 304H specifies a carbon range with a minimum and a relatively coarse grain size (ASTM No. 7 or coarser for austenitic H grades). Standard 304 has no carbon minimum; a 0.02% C heat meeting 304 chemistry may be unsuitable for long-term high-temperature design.
In short: 304L favors corrosion resistance after welding; 304H favors elevated-temperature strength; 304 is the general-purpose grade without a carbon floor.
Comparison: Type 304, 304L and 304H under ASTM A240
The following comparison reflects ASTM A240/A240M flat-rolled limits as commonly tabulated, with Type 304 carbon set to the A240-23 value (user-verified). Values are weight percent; single values are maxima unless a range is shown. Always confirm against the edition of A240/A240M cited on the mill test certificate.
| Grade (Type) | UNS | Carbon (A240-23) | Cr (A240 flat) | Ni (A240 flat) | Notes |
|---|---|---|---|---|---|
| 304 | S30400 | 0.08% max | 17.5–19.5% (18.0–20.0% in some sources) | 8.0–10.5% (8.0–11.0% in one circulated copy) | General-purpose; no C minimum; N 0.10% max; C confirmed against A240-23 |
| 304L | S30403 | 0.030% max | 17.5–19.5% (18.0–20.0% in some sources) | 8.0–12.0% | Low-carbon; preferred for welded corrosive service; N 0.10% max |
| 304H | S30409 | 0.04–0.10% | 18.0–20.0% | 8.0–10.5% | High-carbon; grain size ASTM No. 7 or coarser; no 0.10% N maximum |
Important caveats on published carbon figures
-
Type 304 under A240-23: 0.08% C max. Per ASTM A240/A240M-23 (confirmed against A240-23; user-verified), Type 304 (S30400) carbon is 0.08% max. Do not present 0.07% as the current A240-23 value: that figure appears in EN 1.4301 / ISO 15510 X5CrNi18-10, some older or harmonized association tables (for example BSSA summaries aligned with European flat-product chemistry), and older secondary tabulations—not as the A240-23 Type 304 limit. Chromium and nickel for A240 flat 304 remain as commonly tabulated (Cr 17.5–19.5%, Ni 8.0–10.5% in many association summaries; some circulated copies list Cr 18.0–20.0% and Ni 8.0–11.0%); only carbon was re-verified for this update. This article does not replace the official ASTM document; cite the edition shown on the mill test certificate.
-
Older AISI values. The historic AISI compositions (originally published in the AISI Steel Products Manual and reproduced, for example, in the Nickel Institute guide Design Guidelines for the Selection and Use of Stainless Steels) give 0.08% C max for Type 304 and 0.030% C max for Type 304L, with Cr 18.00–20.00% and Si 1.00% max. The AISI type table in that guide does not list a 304H composition; the same guide notes that the “H” modifications, which set a minimum carbon level, were established by ASTM. The commonly quoted 304H range of 0.04–0.10% C is therefore an ASTM (and ASME) product-specification limit rather than a verified AISI table value. The composition limits in the current edition of SAE J405 (Chemical Compositions of SAE Wrought Stainless Steels) could not be verified from a freely available source for this article.
-
Type 304L: 0.030% versus 0.035%. Under A240 flat-rolled chemistry, 304L is listed as 0.030% C max. Pipe and tube standards such as ASTM A312 and A213 allow 0.035%, and up to 0.040% for small-diameter or thin-wall product that requires many drawing passes. A single “304L = 0.035% C” figure stated without naming the product standard therefore mixes flat-rolled and tubular rules.
-
Type 304H appears as 0.04–0.10% C across A240, A312 and A213; the defining feature is the minimum carbon, not only the maximum. European and ISO near-equivalents do not use exactly the same range (see the next section).
Mechanical property floors also differ slightly: under A240, Type 304 and 304H share higher minimum tensile/yield values than 304L (515 MPa / 205 MPa versus 485 MPa / 170 MPa in common tabulations). Mills frequently produce dual-certified 304/304L heats that meet both the low carbon of 304L and the strength of 304.
SAE 304 Composition Across Standards
The table below compares the chemical composition limits of Type 304 and, where relevant, its low-carbon (304L) and high-carbon (304H) counterparts across major American, European, Japanese, Chinese and international standards. Values are weight percent (cast or heat analysis). Single values are maxima unless a range is given; “n.s.” means no limit is given for that element in the source consulted; “n.v.” means the value could not be verified; “—” means the standard has no corresponding grade. Each row is compiled from the secondary sources listed in Sources and Further Reading; where sources disagree, the disagreement is noted.
| Standard (product form) | Designation | C | Mn | Si | P | S | Cr | Ni | N | Other / notes |
|---|---|---|---|---|---|---|---|---|---|---|
| AISI (historic Steel Products Manual composition) | 304 | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.00–20.00 | 8.00–10.50 | n.s. | Reference composition, not a product specification [9] |
| AISI | 304L | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 18.00–20.00 | 8.00–12.00 | n.s. | [9] |
| AISI | 304H | — | — | — | — | — | — | — | — | Not in the AISI type table consulted; H grades established by ASTM [9] |
| SAE J405 (current edition) | 30304 / 30304L | n.v. | n.v. | n.v. | n.v. | n.v. | n.v. | n.v. | n.v. | n.v. = not verified; current J405 values not checked against a freely available source |
| ASTM A240/A240M-23 (plate, sheet, strip) | 304 (S30400) | 0.08 | 2.00 | 0.75 | 0.045 | 0.030 | 17.5–19.5 | 8.0–10.5 | 0.10 | C 0.08% max confirmed against A240-23 (user-verified); EN/ISO still use 0.07 where applicable; Cr/Ni as commonly tabulated (see caveat 1) [2][3] |
| ASTM A240/A240M | 304L (S30403) | 0.030 | 2.00 | 0.75 | 0.045 | 0.030 | 17.5–19.5 | 8.0–12.0 | 0.10 | Some database entries for earlier editions list Cr 18.0–20.0 [3][17] |
| ASTM A240/A240M | 304H (S30409) | 0.04–0.10 | 2.00 | 0.75 | 0.045 | 0.030 | 18.0–20.0 | 8.0–10.5 | n.s. | Grain size ASTM No. 7 or coarser [2] |
| ASTM A276/A276M (bar, shapes) | 304 (S30400) | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–11.0 | n.s. | [3] |
| ASTM A276/A276M | 304L (S30403) | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–12.0 | n.s. | 304H bar values not verified [3] |
| ASTM A312/A312M (pipe) | TP304 (S30400) | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–11.0 | n.s. | [10][11] |
| ASTM A312/A312M | TP304L (S30403) | 0.035 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–13.0 | n.s. | C 0.040 max for small-OD or thin-wall product needing many drawing passes [10][11] |
| ASTM A312/A312M | TP304H (S30409) | 0.04–0.10 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–11.0 | n.s. | [10] |
| ASTM A213/A213M, ASME SA-213 (seamless boiler and heat-exchanger tube) | TP304 (S30400) | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–11.0 | n.s. | One summary gives P 0.040; not confirmed against the official text [12] |
| ASTM A213/A213M, ASME SA-213 | TP304L (S30403) | 0.035 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–12.0 | n.s. | 0.040 C reported for small-diameter or thin-wall tube [12] |
| ASTM A213/A213M, ASME SA-213 | TP304H (S30409) | 0.04–0.10 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0–20.0 | 8.0–11.0 | n.s. | Grain size ASTM No. 7 or coarser [12] |
| EN 10088-2:2024 (flat products, general purposes) | 1.4301 (X5CrNi18-10) | 0.07 | 2.00 | 1.00 | 0.045 | 0.015 | 17.5–19.5 | 8.0–10.5 | 0.11 | Controlled S ranges permitted for machinability or weldability; one database summary gives N 0.10 [4][5] |
| EN 10088-2:2024 | 1.4307 (X2CrNi18-9), 304L | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 | 17.5–19.5 | 8.0–10.5 | 0.11 | [4] |
| EN 10088-2:2024 | 1.4306 (X2CrNi19-11), 304L | 0.030 | 2.00 | 1.00 | 0.045 | 0.015 | 18.0–20.0 | 10.0–12.0 | 0.11 | Higher-Ni 304L alternative [4] |
| EN (not in EN 10088-2; values from EN 10088-1:2005-based table) | 1.4948 (X6CrNi18-10), 304H-type | 0.04–0.08 | 2.00 | 1.00 | 0.035 | 0.015 | 17.0–19.0 | 8.0–11.0 | 0.11 | Carbon ceiling lower than ASTM 304H; check EN 10028-7 or EN 10216-5 as applicable [5] |
| JIS G4304 (hot-rolled) / G4305 (cold-rolled) | SUS304 | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.00–20.00 | 8.00–10.50 | n.s. | [13][14][15] |
| JIS G4304 / G4305 | SUS304L | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 18.00–20.00 | 9.00–13.00 | n.s. | Ni minimum higher than ASTM 304L [13][14][17] |
| GB/T 4237-2015 (hot-rolled plate, sheet, strip) | 06Cr19Ni10 (S30408), 304 | 0.07 | 2.00 | 0.75 | 0.045 | 0.030 | 17.50–19.50 | 8.00–10.50 | 0.10 | GB/T 4237-2007 listed C 0.08 and Cr 18.00–20.00 [16][19] |
| GB/T 4237-2015 | 022Cr19Ni10 (S30403), 304L | 0.030 | 2.00 | 0.75 | 0.045 | 0.030 | 17.50–19.50 | 8.00–12.00 | 0.10 | [17] |
| GB/T 4237-2015 | 07Cr19Ni10 (S30409), 304H | 0.04–0.10 | 2.00 | 0.75 | 0.045 | 0.030 | 18.00–20.00 | 8.00–10.50 | n.s. | [18] |
| ISO 15510:2014 (composition list, not a product standard) | X5CrNi18-10 (4301-304-00-I) | 0.07 | 2.00 | 1.00 | 0.045 | 0.030 | 17.5–19.5 | 8.0–10.5 | 0.10 | S and Ni carry footnotes not reproduced here [6] |
| ISO 15510:2014 | X2CrNi18-9 (4307-304-03-I), 304L | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 17.5–19.5 | 8.0–10.5 | 0.10 | [6] |
| ISO 15510:2014 | X7CrNi18-9 (4948-304-09-I), 304H | 0.04–0.10 | 2.00 | 1.00 | 0.045 | 0.030 | 17.5–19.5 | 8.0–11.0 | 0.10 | [6] |
Numbers in brackets refer to the numbered items in Sources and Further Reading.
Observations
- Two families of 304 chemistry. ASTM A240-23 Type 304 uses C ≤ 0.08% (user-verified against A240-23). EN 10088-2, ISO 15510 and GB/T 4237-2015 generally still use C ≤ 0.07%, Cr 17.5–19.5% for standard 304. Long-product and tubular ASTM standards (A276, A312, A213), the historic AISI composition and JIS SUS304 also use C ≤ 0.08%, Cr 18.0–20.0%. Association tables that list A240 304 as 0.07% C are EN/ISO-aligned summaries, not the A240-23 value.
- Silicon and sulfur. Si is 0.75% max in A240 and GB/T 4237 but 1.00% max in the bar, pipe, tube, EN, JIS and ISO entries. EN 10088-2 sets a lower base sulfur limit (0.015%) than the ASTM, JIS and GB/T standards (0.030%).
- Nitrogen. A240, GB/T 4237-2015 and ISO 15510 cap N at 0.10% for 304 and 304L; EN 10088-2 gives 0.11% (according to BSSA’s summary of the 2024 edition). The pipe, tube, bar and JIS entries list no nitrogen limit for these grades.
- 304L nickel. The upper nickel limit for 304L varies widely: 10.5% (EN 1.4307, ISO X2CrNi18-9), 12.0% (A240, A276, A213, GB/T, EN 1.4306) and 13.0% (A312, JIS SUS304L). JIS SUS304L also has a higher minimum (9.00%).
- 304H carbon. ASTM, GB/T and ISO use 0.04–0.10% C, while the European 1.4948 entry uses 0.04–0.08%.
Verification note: The values above are compiled from association publications, standards previews and published standards summaries, not from purchased copies of each standard—except ASTM A240-23 Type 304 carbon (0.08% max), which was confirmed against A240-23 (user-verified). Composition limits change between editions (for example GB/T 4237-2007 to -2015, and EN 10088-2:2005 to -2014 to -2024). Verify every value against the official, current edition of the relevant standard before using it for purchasing, design or certification.
Flat-Rolled (A240) Versus Pipe, Tube and Bar
Consistent with the comparison table above, composition limits for the “same” grade change with product form:
| Product form | Typical ASTM specification | Type 304 carbon | Type 304L carbon | Type 304H carbon |
|---|---|---|---|---|
| Plate, sheet, strip | A240 / A240M (ASME SA-240) | 0.08% max (A240-23, user-verified) | 0.030% max | 0.04–0.10% |
| Seamless and welded pipe | A312 / A312M (ASME SA-312) | 0.08% max | 0.035% max (0.040% for small-OD or thin-wall product) | 0.04–0.10% |
| Seamless boiler, superheater and heat-exchanger tube | A213 / A213M (ASME SA-213) | 0.08% max | 0.035% max (0.040% reported for small-diameter or thin-wall tube) | 0.04–0.10% |
| Bars and shapes | A276 / A276M | 0.08% max | 0.030% max | not verified |
Chromium and silicon limits also shift with product form: A312, A213 and A276 list Cr 18.0–20.0% and Si 1.00% max for 304, whereas harmonized A240 tables list Cr 17.5–19.5% and Si 0.75% max. Nickel ceilings for 304L range from 12.0% (A240, A213, A276) to 13.0% (A312).
The National Board and pressure-equipment literature note that tubes (e.g., SA-213), pipes (e.g., SA-312 and SA-376) and plates (SA-240) each carry slightly different composition ranges even when the grade name is “304.” ASSDA likewise states that specifications for some other products, particularly tube and pipe, use a carbon limit of 0.035% or 0.040% maximum for 304L while remaining otherwise similar.
The precise statement is therefore: carbon maxima for Types 304 and 304L depend on the product specification; ASTM A240-23 Type 304 is 0.08% C max (same ceiling as A312/A213 for TP304), but 304L remains 0.030% max under A240 versus 0.035% (or 0.040% for small-OD/thin-wall) under A312/A213. Citing a single “304L = 0.035% C” figure without naming the standard is incomplete. EN/ISO near-equivalents still use 0.07% C max for 1.4301 / X5CrNi18-10.
Typical Chromium and Nickel Ranges (304 Family, A240)
Within the A240 flat-rolled family, chromium and nickel stay in the classic “18-8” window:
- Chromium: about 17.5–19.5% for 304 and 304L in harmonized flat-product tables; 18.0–20.0% for 304H and in some older or alternative A240 tabulations.
- Nickel: about 8.0–10.5% for 304; 8.0–12.0% for 304L; 8.0–10.5% for 304H.
- Other controlled elements include Mn (2.00% max), Si (0.75% max in A240), P (0.045% max), S (0.030% max) and, for the standard and L grades, nitrogen at 0.10% max.
These are specification envelopes, not a catalogue of finishes or thicknesses.
Brief Applications by Grade
Type 304. General use in atmospheric, food-contact, architectural and mildly corrosive chemical environments; formed sheet; parts that are not heavily welded in corrosive service. Chosen for a balance of formability, toughness and corrosion resistance.
Type 304L. Welded tanks, process equipment, piping and fabrications where post-weld solution annealing is impractical and intergranular corrosion is a concern. Often dual-certified with 304 when both low carbon and 304-level strength are required.
Type 304H. Elevated-temperature pressure equipment and heaters where creep and stress-rupture strength govern design. Not preferred for aqueous corrosion after prolonged sensitization-range exposure unless that risk is acceptable.
Code vessels and piping must follow the applicable ASME/ASTM product specification and allowable-stress tables, not grade name alone.
Sources and Further Reading
Primary and secondary references (verify edition dates; do not treat unofficial PDF copies as authoritative):
- ASTM International, A240/A240M: Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications, product page: https://www.astm.org/a0240_a0240m-23.html. Purchase or access the current
Disclaimer: Figures above are compiled from association summaries, standards previews and published standards summaries. ASTM A240-23 Type 304 carbon is 0.08% max (user-verified against A240-23); the 0.07% figure belongs to EN/ISO and some older harmonized tables, not current A240-23. Only the official text of the cited standard and edition governs contractual and Code compliance.
Related product data (separate from technical claims above)
For mill-oriented flat-product data sheets related to A240 Type 304L sheet and plate, see: ASTM A240 Type 304L stainless steel sheet/plate. This product page is not part of the technical claims above and need not be cited for encyclopedic references.