GB/T 19879 Q500GJC Building Steel Plate Supplier
What is GB/T 19879 Q500GJC Building Steel Plate?
Q500GJC, also written Q500GJ-C or Q500 GJC, is high-strength plate for building structures under GB/T 19879-2023. Q means yield, 500 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and C is the quality grade: Charpy V-notch at 0°C, at least 55 J.
The GJ rules still apply at this strength. Q500GJC has a yield ceiling of 640 MPa above 20 mm, a CEV cap of 0.52% for QT plate and low P and S. Unlike Q235GJ–Q460GJ, it is made only by quenching and tempering or TMCP, only from 12 to 50 mm, and its yield ratio is agreed in the contract.
Q500GJC is the first of the four high-strength GJ grades. It is not hot-rolled GJ plate pushed harder: it is quenched and tempered or TMCP plate, 12–50 mm thick, with its own CEV limits. The C letter here needs 55 J at 0°C, more energy than the D and E letters ask for.
GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. Q500GJ entered GB/T 19879 in the 2015 edition; the 2005 edition stopped at Q460GJ. In 2015 the grade covered 12–40 mm and reported ReL. The 2023 edition keeps the same chemistry, extends the range to 50 mm, reports ReH, and sets 55 J at 0°C for C and 47 J at −20°C / −40°C for D and E. Sister grades are listed under GB/T 19879, including Q500GJD.
SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q500GJC cut to size with an EN 10204 3.1 or 3.2 certificate.
Material Specification
| Specification element | Requirement | SHH STEEL compliance |
|---|---|---|
| Plate standard | GB/T 19879-2023 Q500GJC (GB/T 19879-2015 when the drawing names it) | Confirmed |
| Thickness for Q500GJ | 12 mm – 50 mm | Confirmed |
| Yield strength | 500 MPa min; 500 – 640 MPa above 20 mm | Confirmed |
| Tensile strength | 610 – 770 MPa | Confirmed |
| Yield ratio | By agreement; we print it on the MTC | Printed on MTC |
| Quality grade | C, Charpy V at 0°C, KV2 ≥ 55 J, longitudinal | Confirmed |
| Delivery condition | QT, TMCP or TMCP+T | As ordered |
| Through-thickness | Z15, Z25 or Z35 to GB/T 5313 | As ordered |
| Dimensions | GB/T 709-2019, thickness tolerance Class B | Confirmed |
| Chemistry report | Heat analysis + CEV; product analysis on request | Confirmed |
| Certificate | EN 10204 3.1 or 3.2 | As ordered |
Grades often confused with it are GB/T 16270 Q500C and GB/T 1591 Q500MC. None of them carries the GJ yield cap.
Chemical Composition: Heat Analysis and Product Analysis
Two chemistry numbers exist for every Q500GJC plate. The mill reports the heat (ladle) analysis, which must sit inside Table 1. A check analysis drilled from the plate is the product analysis; clause 7.1.4 of GB/T 19879 lets it differ from Table 1 by the GB/T 222 deviations.
Table 1 below is the heat analysis for Q500GJC. The columns on the right show the quality-grade groups at Q500GJ.
Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %
| Element | Q500GJC heat analysis (%) | Q500GJ C | Q500GJ D / E |
|---|---|---|---|
| C, max | 0.18 | 0.18 | 0.18 |
| Si, max | 0.60 | 0.60 | 0.60 |
| Mn, max | 1.80 | 1.80 | 1.80 |
| P, max | 0.025 | 0.025 | 0.020 |
| S, max | 0.015 | 0.015 | 0.010 |
| V, max | 0.120 | 0.120 | 0.120 |
| Nb, max | 0.110 | 0.110 | 0.110 |
| Ti, max | 0.030 | 0.030 | 0.030 |
| Als, min | 0.015 | 0.015 | 0.015 |
| Cr, max | 1.20 | 1.20 | 1.20 |
| Cu, max | 0.50 | 0.50 | 0.50 |
| Ni, max | 1.20 | 1.20 | 1.20 |
| Mo, max | 0.60 | 0.60 | 0.60 |
| B, max (if added) | 0.003 | 0.003 | 0.003 |
Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. When boron is added, and for any QT plate, B ≤ 0.003%. These limits are the same in the 2015 and 2023 editions.
The C and D/E columns differ only in P and S: the D and E letters tighten P to 0.020% and S to 0.010%. Carbon stays at 0.18% for every quality letter at this level.
Table 2. Product analysis limits for Q500GJC, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %
| Element | Heat limit (%) | Permitted deviation, GB/T 222-2025 Table 2 (alloy steel) | Q500GJC product analysis limit (%) |
|---|---|---|---|
| C | ≤ 0.18 | +0.01 | ≤ 0.19 |
| Si | ≤ 0.60 | +0.04 | ≤ 0.64 |
| Mn | ≤ 1.80 | +0.04 | ≤ 1.84 |
| P | ≤ 0.025 | +0.005 | ≤ 0.030 |
| S | ≤ 0.015 | +0.005 | ≤ 0.020 |
| V | ≤ 0.120 | +0.03 | ≤ 0.150 |
| Nb | ≤ 0.110 | Agree in contract | Agree in contract |
| Ti | ≤ 0.030 | +0.02 | ≤ 0.050 |
| Als | ≥ 0.015 | ±0.005 band (Al ≤ 0.10%) | Agree in contract |
| Cr | ≤ 1.20 | +0.05 | ≤ 1.25 |
| Cu | ≤ 0.50 | +0.03 | ≤ 0.53 |
| Ni | ≤ 1.20 | +0.05 | ≤ 1.25 |
| Mo | ≤ 0.60 | +0.02 | ≤ 0.62 |
| B (if added) | ≤ 0.003 | Agree in contract | Agree in contract |
How to read Table 2. Q500GJ–Q690GJ heats carry Ni, Cr, Mo and often B for hardenability, which normally classes them as alloy steel, so the alloy-steel table of GB/T 222 applies. For Q500GJC, Mn ≤1.80% sits in the 1.00–2.00% band (±0.04), and Ni ≤1.20% in the 1.00–2.00% band (±0.05). GB/T 222 clause 5.4 says one steel uses one table only, so the certificate should state which table was applied.
GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).
Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.
Mechanical Properties
Values below follow Table 4 and Table 5 of GB/T 19879-2023 for Q500GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.
| Thickness | Upper yield ReH (MPa) | Tensile Rm (MPa) | Yield ratio, max | Elongation A, min |
|---|---|---|---|---|
| 12 – 20 mm | ≥ 500 | 610 – 770 | By agreement | 17% |
| > 20 – 50 mm | 500 – 640 | 610 – 770 | By agreement | 17% |
Below 20 mm only the 500 MPa minimum applies; from 20 to 50 mm the 500 – 640 MPa window applies. Write the yield-ratio limit into the contract; GB/T 19879-2023 leaves it to agreement for this grade.
| Test | Q500GJC requirement |
|---|---|
| Charpy V-notch, longitudinal | 0°C, KV2 ≥ 55 J, average of 3 |
| Single value | One value may fall below the average requirement, not below 70% of it (GB/T 17505) |
| Sub-size specimens | 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy |
| 180° bend | Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2) |
| Through-thickness (≥ 15 mm) | Z15, Z25 or Z35 to GB/T 5313, when ordered |
Density for theoretical weight is 7.85 g/cm³.
Q500GJC vs S500Q and GB/T 16270 Q500C: What Building Plate Adds
At 500 MPa the plate itself is not unusual. GB/T 16270 Q500C and EN 10025-6 S500Q are standard QT products. What Q500GJC adds is a building-steel frame around them: a yield ceiling of 640 MPa above 20 mm, a tensile floor of 610 MPa, a CEV cap written into the standard, and Charpy at the GB quality letter.
The trade-off is thickness. GB/T 19879 stops at 50 mm for this grade; EN 10025-6 and GB/T 16270 go much thicker.
| Property | S500Q (EN 10025-6) | Q500C (GB/T 16270) | Q500GJC (GB/T 19879-2023) |
|---|---|---|---|
| Delivery | QT | QT | QT or TMCP |
| Thickness range | to 150 mm | to 150 mm | 12 – 50 mm |
| Yield, ≤ 50 mm | ≥ 500 MPa | ≥ 500 MPa | 500 – 640 MPa above 20 mm |
| Tensile, ≤ 50 mm | 590 – 770 MPa | Per GB/T 16270 | 610 – 770 MPa |
| Yield ratio | No limit | No limit | By agreement (write it on the order) |
| Impact | 0°C / −20°C (Q) | 0°C | 0°C, 55 J |
| Elongation A | 17% | Per GB/T 16270 | 17% |
| CEV ≤ 50 mm | Per EN 10025-6 | Per GB/T 16270 | 0.52% QT / 0.47% TMCP |
If a member is thicker than 50 mm, it cannot be Q500GJC. The designer either splits the plate, or moves to GB/T 16270 Q500C or the EN grade with project-specific yield-cap rules. The TMCP comparison in GB/T 1591 is GB/T 1591 Q500MC.
QT or TMCP? Delivery Condition, CEV and Weldability of Q500GJC
| Route | CEV max (≤ 50 mm) | Pcm max (≤ 50 mm) | Typical use |
|---|---|---|---|
| QT (incl. direct quench) | 0.52% | By agreement | Full strength through 50 mm; highest alloy |
| TMCP, TMCP+T | 0.47% | 0.28% (reference value) | Leaner chemistry; easier welding on thinner plate |
Q500GJ cannot be made as plain hot-rolled or normalized plate; GB/T 19879-2023 lists only QT and TMCP routes for it. The two routes are not equal at the welding bay.
QT Q500GJC carries up to 0.52% CEV, because the mill adds Mn, Ni, Cr, Mo and sometimes B for hardenability. TMCP plate is capped at 0.47%. For welding procedure purposes those are different steels.
The 2023 edition lets TMCP plate ship against Pcm instead of CEV only when buyer and mill agree in the contract. The Pcm figure in the standard for TMCP plate is given for reference.
Q500GJC, Q500GJD or Q500GJE: Which Quality Grade?
| Grade | Impact temperature | Energy, min | C / P / S max (%) | Typical use |
|---|---|---|---|---|
| Q500GJC | 0°C | 55 J | 0.18 / 0.025 / 0.015 | Cold regions, exposed frames |
| Q500GJD | −20°C | 47 J | 0.18 / 0.020 / 0.010 | Severe winters, thick welded nodes |
| Q500GJE | −40°C | 47 J | 0.18 / 0.020 / 0.010 | Arctic and low-temperature sites |
Strength, yield window and CEV do not change from C to E. Only the impact temperature, the C-grade energy (55 J) and the D/E P and S limits move. The letter should follow the coldest temperature the steel will see, during erection as well as in service.
Q500GJC is the usual letter for temperate sites and for frames that see some frost during erection. For the same letter at another strength level: one level up, Q550GJC; one level down, Q460GJC.
Q500GJCZ15, Q500GJCZ25 and Q500GJCZ35: Through-Thickness Plate
Lamellar tearing starts inside the plate, parallel to the surface, when a large weld pulls on it through the thickness. Box-column diaphragms and T-joints on thick flanges are the classic cases. A Z grade is the guarantee against it.
The designation adds the Z level to the grade, for example Q500GJCZ25. Z tests apply to plate 15–50 mm and follow GB/T 5313-2023.
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
B and C chemistry allows S up to 0.015%, so even Z15 needs extra desulfurization.
GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.
Our advice: mark Z25 or Z35 on the cutting list by member, not on the whole order. Stiffeners and webs rarely need it.
Equivalent Material Grades
At 500 MPa every foreign comparison is a QT plate standard, not a building-steel standard. They match strength and toughness temperature. None of them sets a yield ceiling or a yield-ratio rule.
| Designation | Region | Standard | Notes |
|---|---|---|---|
| Q500GJC | China | GB/T 19879-2023 | Grade on this page; 12–50 mm |
| EN 10025-6 S500Q | Europe | EN 10025-6 | QT; closest strength match |
| EN 10025-6 S500QL | Europe | EN 10025-6 | Colder sub-grade |
| GB/T 16270 Q500C | China | GB/T 16270 | QT structural plate; thicker sizes |
| GB/T 1591 Q500MC | China | GB/T 1591-2018 | TMCP route |
| ASTM A709 HPS 70W | USA | ASTM A709 | 485 MPa; one step lower |
See EN 10025-6 and GB/T 16270 for thicker or non-building QT plate.
Weldability
GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q500GJC certificate:
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B
| Delivery condition | CEV, max (≤ 50 mm) | Pcm, max (≤ 50 mm) |
|---|---|---|
| QT (quenched + tempered, incl. direct quench) | 0.52 | By agreement |
| TMCP, TMCP+T | 0.47 | 0.28 (for reference) |
Q500GJ plate is high-strength steel and is welded like it: low-hydrogen consumables, measured preheat, interpass limits and a heat-input window that protects the tempered structure.
The impact test on the C letter is at 0°C. Qualify the HAZ Charpy at that temperature, not only the weld metal.
Typical consumables: E62-class low-hydrogen electrodes (GB/T 5118 E6215 types) or matching wire. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.
Heat Treatment and Delivery Condition
Q500GJC is delivered QT (quenched and tempered, including in-line direct quenching) or TMCP / TMCP+T. Hot-rolled and normalized delivery are not allowed for this grade.
Most building orders at this level ship QT. TMCP plate is possible on thinner sizes and gives a lower CEV cap, but not every mill can hold the GJ yield ceiling on TMCP plate up to 50 mm.
Tempering temperature and time are mill data. We ask for them on the MTC when the fabricator plans post-weld heat treatment, so that PWHT stays below the tempering temperature. QT references: GB/T 16270 Q500C and EN 10025-6 S500Q.
Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.
Dimensions
Q500GJC sizes we supply from mill and stock:
- Thickness: 12 mm – 50 mm
- Width: 1500 mm – 3000 mm standard; wider by mill confirmation; QT width depends on the mill’s quench line
- Length: 3000 mm – 12000 mm; longer by enquiry
- Edge: mill edge or cut edge
- Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³
Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.
Tolerances
Dimensional tolerances for Q500GJC come from GB/T 709-2019, as GB/T 19879 directs. The default is Class B, which fixes the minus side at 0.30 mm. Ask for Class C if the design cannot accept any minus.
| Nominal thickness (mm) | Width ≤ 1500 mm | Width > 1500 – 2500 mm |
|---|---|---|
| > 8 – 15 | −0.30 / +0.80 | −0.30 / +1.00 |
| > 15 – 25 | −0.30 / +1.00 | −0.30 / +1.20 |
| > 25 – 40 | −0.30 / +1.10 | −0.30 / +1.30 |
| > 40 – 60 | −0.30 / +1.30 | −0.30 / +1.50 |
Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.
Supplementary Requirements
Q500GJC already fixes strength, yield window, CEV and 0°C impact. Anything more goes on the purchase order.
- Edition: GB/T 19879-2023 or -2015. Never write only Q500.
- Product analysis: ask for a second chemistry column checked to GB/T 222.
- Through-thickness: add Z15, Z25 or Z35, e.g. Q500GJCZ25.
- Delivery route: QT or TMCP, and the CEV/Pcm basis.
- Yield ratio: the designer’s limit, since the standard leaves it to agreement.
- Tempering data on the MTC if the fabricator plans post-weld heat treatment.
- Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the C letter.
- Tolerance: Class C for zero minus.
- Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.
Q500GJC Price Factors and How to Order
Two Q500GJC quotes can differ by a lot and both be fair. The base price is similar across mills; the extras below are where they part.
| Cost driver | Effect on price |
|---|---|
| GJ grade over general Q500 plate | Grade extra for cleaner steel, yield control and CEV |
| Quality letter C | Extra for 55 J at 0°C |
| Delivery route | QT line time is the main cost driver at this level |
| Thickness | 12–20 mm and 40–50 mm carry the most care; 20–40 mm is the core range |
| Z15 / Z25 / Z35 | Desulfurization, plate-by-plate Z test and UT; Z35 costs most |
| Width and length | Over 3000 mm wide or 12 m long needs mill confirmation |
| Quantity per size | Mill rolling minimums per size; small lots come from stock or combined rolling |
| Inspection and cutting | 3.2 witness, profile cutting, blasting and priming are quoted per item |
To get a firm quote in one round, send:
- Grade and edition, e.g. Q500GJCZ25 to GB/T 19879-2023
- Thickness × width × length and pieces or tonnes
- Delivery route, UT standard and class
- Certificate type and inspector
- Destination port and Incoterm
We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q500GJE.
Applications
| Sector | Typical Q500GJC components |
|---|---|
| Long-span roofs | Compression chords and diagonals where weight governs |
| Tall buildings | Outrigger and belt truss members, hanger plates |
| Heavy industrial buildings | Crane-runway and support members |
| Special structures | Members where crane capacity or connection size limits plate thickness |
C grade suits frames that see winter during erection or in service, and exposed members in temperate climates.
It is not boiler or pressure-vessel plate (pressure vessel steel plates), and members thicker than 50 mm move to GB/T 16270 or EN 10025-6.
Supply Capability and Global Delivery
SHH STEEL sources Q500GJC from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Valin Xiangtan and Shougang QT lines.
- Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
- Tests: tensile, 0°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
- Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
- Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
- Marking: steel-stamped and paint-marked with grade, heat, size and mill
Q500GJC leaves Shanghai for projects designed to Chinese codes abroad, mostly through EPC contractors in Southeast Asia, the Middle East and Africa. We also ship ASTM, ASME, EN, DIN and JIS plate to Europe and the Americas.
QT plate is rolled and heat treated to order: about 45–60 days; 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.
Why Choose SHH STEEL
SHH STEEL works mill-direct as a steel manufacturer and exporter and global steel mill sourcing partner, China origin. With Q500GJC you get the GJ plate the drawing asks for, traced to the heat.
Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio inside the agreed limit, CEV inside the thickness band for the delivery route, and 0°C impact at 55 J or more. If one fails, the plate does not ship as GJ.
We also tell buyers when they are over-specifying. If a member is thicker than 50 mm, we tell you before quoting: it cannot be Q500GJC. Browse more structural steel plates and high strength low alloy plates.
FAQ
-
What is Q500GJC steel?
- Q500GJC is high-strength building structure steel plate to GB/T 19879-2023, delivered quenched and tempered or TMCP in 12–50 mm. It has 500 MPa minimum yield, 500–640 MPa yield above 20 mm, 610 – 770 MPa tensile, a CEV cap of 0.52% (QT) and Charpy impact of at least 55 J at 0°C.
-
What is the difference between Q500GJC and S500Q?
- S500Q (EN 10025-6) is QT plate with ≥500 MPa yield up to 50 mm, no yield ceiling and no yield-ratio rule, made to 150 mm. Q500GJC (GB/T 19879-2023) is QT or TMCP building plate, 12–50 mm, with 500–640 MPa yield above 20 mm, 610 – 770 MPa tensile, a CEV cap of 0.52% (QT) and 55 J at 0°C.
-
Why does Q500GJC need 55 J when the D and E grades need 47 J?
- GB/T 19879-2023 Table 5 sets 55 J at 0°C for grade C of Q500GJ to Q690GJ, and 47 J at −20°C (D) and −40°C (E). The C requirement is a higher energy at a warmer temperature. A D-grade certificate tested only at −20°C has not proven 55 J at 0°C, so state the letter you need.
-
Is Q500GJ quenched and tempered?
- Q500GJ is delivered either quenched and tempered (including direct quenching) or TMCP/TMCP+T; GB/T 19879-2023 lists no hot-rolled or normalized route for it. CEV is capped at 0.52% for QT plate and 0.47% for TMCP plate.
-
What is the CEV limit of Q500GJC?
- For Q500GJC up to 50 mm, CEV is capped at 0.52% for QT plate and 0.47% for TMCP plate, under GB/T 19879-2023 Table 2. CEV is calculated from the heat analysis: C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15.
-
What is the ASTM or EN equivalent of Q500GJC?
- The closest European grade is EN 10025-6 S500Q; the closest Chinese non-building grades are GB/T 16270 Q500C (QT) and GB/T 1591 Q500MC (TMCP). They match strength only: Q500GJC adds a 640 MPa yield ceiling, a CEV cap and a 50 mm thickness limit.
Conclusion
Q500GJC steel plate to GB/T 19879 is building structure plate with 500 MPa minimum yield, a capped yield window, a yield ratio agreed in the contract and 55 J impact at 0°C. It shares its chemistry with Q500GJD but proves toughness at its own letter. It is not general structural plate under GB/T 1591 or GB/T 16270.
Every Q500GJC plate from SHH STEEL ships with heat analysis, CEV, yield and yield ratio, and Charpy results on an EN 10204 3.1 or 3.2 certificate. Product analysis to GB/T 222, Z15–Z35, UT to GB/T 2970, Class C tolerance and cut-to-size are options.
We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.
Share your size list, Z level, quality letter and the edition on the drawing, and we reply with the mill, delivery route, lead time, test plan and price in one message. Contact SHH STEEL for a mill-direct Q500GJC building steel plate quotation.