GB/T 19879 Q460GJD building steel plates stacked near cranes at SHH STEEL

GB/T 19879 Q460GJD Building Steel Plate Supplier

GB/T 19879 Q460GJD is high-performance building structure steel plate with 460 MPa minimum yield, a 460 – 590 MPa yield window, yield ratio ≤0.85 and 47 J Charpy impact at −20°C. SHH STEEL supplies Q460GJD mill-direct, 6 mm – 150 mm, with Z15, Z25 or Z35 options and full heat and product analysis.
Keywords
Q460GJD, Q460GJD steel plate, GB/T 19879 Q460GJD, Q460GJ-D, Q460GJDZ15, Q460GJDZ25, Q460GJDZ35, Q460GJ, building structure steel plate, Q460GJD supplier
Equivalent Grades
GB/T 19879 Q460GJD / EN 10025-3 S460N / EN 10025-4 S460M / EN 10025-6 S460Q (strength only) / ASTM A572 Gr.65 / JIS G3106 SM570 — Material Specification: GB/T 19879-2023 (supersedes GB/T 19879-2015) — Delivery: CR, NR, N, NT, QT, TMCP or TMCP+T; −20°C impact
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q460GJD vs S460
N, TMCP or QT?
Material Comparison
Z15 / Z25 / Z35
Equivalent Material Grades
Weldability
Heat Treatment and Delivery Condition
Dimensions
Tolerances
Supplementary Requirements
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 19879 Q460GJD Building Steel Plate?

Q460GJD, also written Q460GJ-D or Q460 GJD, is hot-rolled steel plate for building structures under GB/T 19879. Q means yield, 460 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and D is the quality grade: Charpy V-notch at −20°C, at least 47 J.

The GJ rules are what the structural engineer is paying for. Q460GJD sets a maximum yield as well as a minimum, caps the yield ratio, limits carbon equivalent by thickness and delivery route, and keeps P and S low. The frame then yields where the designer expects.

Q460GJD is the −20°C version for heavy plate in cold regions. At 460 MPa and 100 mm, holding 47 J at −20°C is a mill-process question, so the delivery route (N, TMCP or QT) should be agreed before the price.

GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. Q460GJ got its own CEV and Pcm limits in the 2015 edition. The 2023 edition keeps them, raises the yield-ratio cap from 0.83 to 0.85, uses ReH and holds 460–590 MPa to 100 mm. Chemistry, including Nb up to 0.110%, is unchanged. Sister grades are listed under GB/T 19879, including Q460GJB.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q460GJD cut to size with an EN 10204 3.1 or 3.2 certificate.

Material Specification

Specification element Requirement SHH STEEL compliance
Plate standard GB/T 19879-2023 Q460GJD (GB/T 19879-2015 when the drawing names it) Confirmed
Thickness for Q460GJ 6 mm – 150 mm Confirmed
Yield strength 460 MPa min; 460 – 590 MPa for 16–100 mm Confirmed
Tensile strength 570 – 720 MPa (to 100 mm) Confirmed
Yield ratio ≤ 0.85 Printed on MTC
Quality grade D, Charpy V at −20°C, KV2 ≥ 47 J, longitudinal Confirmed
Delivery condition CR, NR, N, NT, QT, TMCP or TMCP+T As ordered
Through-thickness Z15, Z25 or Z35 to GB/T 5313 As ordered
Dimensions GB/T 709-2019, thickness tolerance Class B Confirmed
Chemistry report Heat analysis + CEV; product analysis on request Confirmed
Certificate EN 10204 3.1 or 3.2 As ordered

Grades often confused with it are GB/T 1591 Q460D and ASTM A572 Gr.65. None of them carries the GJ yield cap or yield-ratio rule.

Chemical Composition: Heat Analysis and Product Analysis

Buyers often reject plate because a third-party lab reads 0.02% more carbon than the MTC. That is usually not a failure. Table 1 is the heat (ladle) limit; plate drilled after rolling is judged as product analysis, with the tolerances of GB/T 222 that clause 7.1.4 calls up.

Table 1 below is the heat analysis for Q460GJD. The columns on the right show the quality-grade groups at Q460GJ.

Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %

Element Q460GJD heat analysis (%) Q460GJ B / C Q460GJ D / E
C, max 0.18 0.20 0.18
Si, max 0.55 0.55 0.55
Mn, max 1.70 1.70 1.70
P, max 0.020 0.025 0.020
S, max 0.010 0.015 0.010
V, max 0.200 0.200 0.200
Nb, max 0.110 0.110 0.110
Ti, max 0.030 0.030 0.030
Als, min 0.015 0.015 0.015
Cr, max 1.20 1.20 1.20
Cu, max 0.50 0.50 0.50
Ni, max 1.20 1.20 1.20
Mo, max 0.50 0.50 0.50
V + Nb + Ti, max (if combined) 0.22 0.22 0.22

Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. V + Nb + Ti, when combined, is limited to 0.22%. These limits are the same in the 2015 and 2023 editions.

B and C grades share one chemistry column. D and E grades tighten carbon to 0.18%, phosphorus to 0.020% and sulfur to 0.010%, because they are tested at −20°C and −40°C.

Table 2. Product analysis limits for Q460GJD, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %

Element Heat limit (%) Permitted deviation, GB/T 222-2025 Table 1 Q460GJD product analysis limit (%)
C ≤ 0.18 +0.02 ≤ 0.20
Si ≤ 0.55 +0.05 ≤ 0.60
Mn ≤ 1.70 +0.06 ≤ 1.76
P ≤ 0.020 +0.005 ≤ 0.025
S ≤ 0.010 +0.005 ≤ 0.015
V ≤ 0.200 +0.02 ≤ 0.220
Nb ≤ 0.110 ±0.005 ≤ 0.115 (Table 1 lists Nb to 0.060%; agree above that)
Ti ≤ 0.030 +0.02 ≤ 0.050
Als ≥ 0.015 −0.003 ≥ 0.012
Cr ≤ 1.20 +0.05 ≤ 1.25
Cu ≤ 0.50 +0.05 ≤ 0.55
Ni ≤ 1.20 +0.05 ≤ 1.25 (Table 1 covers Ni to 1.00%)
Mo ≤ 0.50 Not listed in Table 1 Agree in contract (alloy-steel Table 2 would give ≤ 0.52)

How to read Table 2. The band is chosen by the Table 1 upper limit. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn ≤1.70% falls in the 0.80–1.70% band, so +0.06%. For one heat an element may deviate in one direction only. Ni up to 1.20% is beyond the 1.00% range of Table 1; we apply the alloy-steel figure (±0.05%), which gives the same limit.

GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).

Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.

Mechanical Properties

Values below follow Table 3 and Table 5 of GB/T 19879-2023 for Q460GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.

Thickness Upper yield ReH (MPa) Tensile Rm (MPa) Yield ratio, max Elongation A, min
6 – 16 mm ≥ 460 570 – 720 0.85 18%
> 16 – 100 mm 460 – 590 570 – 720 0.85 18%
> 100 – 150 mm 440 – 570 550 – 700 0.85 18%

The 2015 edition used lower yield ReL and stepped yield down 10 MPa above 50 mm. Write the edition on the order so the mill tests to the right table.

Test Q460GJD requirement
Charpy V-notch, longitudinal −20°C, KV2 ≥ 47 J, average of 3
Single value One value may fall below the average requirement, not below 70% of it (GB/T 17505)
Sub-size specimens 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy
180° bend Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2)
Through-thickness (≥ 15 mm) Z15, Z25 or Z35 to GB/T 5313, when ordered

Density for theoretical weight is 7.85 g/cm³.

Q460GJD vs S460 (N, M and Q): Which 460 MPa Plate Fits a Building Frame?

European engineers reviewing a Chinese tower often ask whether Q460GJD is just S460. It is not. S460N and S460M give 460 MPa on thin plate and step down with thickness; S460Q holds yield longer but has no ceiling. None of them limits the yield ratio.

Q460GJD keeps 460–590 MPa from 16 mm to 100 mm and caps the ratio at 0.85. That is a seismic-design requirement, not a strength upgrade.

Property S460N / S460M S460Q (EN 10025-6) Q460GJD (GB/T 19879-2023)
Delivery Normalized / TMCP Quenched + tempered CR, NR, N, NT, QT or TMCP
Yield at 16 mm 460 MPa 460 MPa 460 MPa
Yield at 40–63 mm 430 MPa min 460 MPa min (to 50 mm) 460 – 590 MPa
Yield at 80–100 mm 400 MPa min 440 MPa min 460 – 590 MPa
Yield upper limit None None 590 MPa to 100 mm
Yield ratio No limit No limit ≤ 0.85
Impact N/M −20°C 40 J; NL/ML −50°C 27 J Q −20°C; QL −40°C; QL1 −60°C −20°C, 47 J

For −20°C, EN 10025-4 S460M (TMCP) and EN 10025-3 S460N (normalized) are the closest. On the GB side, GB/T 1591 Q460ND and GB/T 1591 Q460MD.

Closest single comparison for Q460GJD: EN 10025-4 S460M, strength only.

N, TMCP or QT? Choosing the Delivery Route for Q460GJD

Route (GB/T 19879-2023) CEV ≤ 50 / 50–100 / 100–150 mm Pcm ≤ 50 / 50–100 / 100–150 mm What it means in the shop
CR, NR, N, NT 0.52 / 0.54 / 0.56% 0.32 / 0.34 / 0.35% Highest CEV; more preheat on thick plate
QT 0.45 / 0.48 / 0.50% 0.28 / 0.30 / 0.31% Lower CEV, full-thickness strength; heat-input limits matter
TMCP, TMCP+T 0.42 / 0.45 / by agreement 0.27 / by agreement Lowest CEV; best weldability to 100 mm

The same grade name covers three very different plates. A 100 mm normalized Q460GJD plate can carry CEV 0.54%; a TMCP plate of the same thickness, 0.45%. The fabricator’s preheat, interpass and consumable choice follow that number.

We put the route on the quotation. If the drawing is silent, we recommend TMCP up to about 80 mm and QT for the heaviest plate, then let the welding engineer confirm.

Q460GJB, Q460GJC, Q460GJD or Q460GJE: Which Quality Grade?

Grade Impact temperature Energy, min C / P / S max (%) Typical use
Q460GJB +20°C 47 J 0.20 / 0.025 / 0.015 Heated interiors, mild climates
Q460GJC 0°C 47 J 0.20 / 0.025 / 0.015 Cold regions, exposed frames
Q460GJD −20°C 47 J 0.18 / 0.020 / 0.010 Severe winters, thick welded nodes
Q460GJE −40°C 47 J 0.18 / 0.020 / 0.010 Arctic and low-temperature sites

Strength, yield ratio and CEV do not change from B to E. Only the impact temperature and the D/E chemistry move. Choose the letter from the site climate and plate thickness, not from habit.

Q460GJD is the letter for −20°C design temperatures, and the one we suggest when the plate is thick and restrained. For the same letter at another strength level: one level up, Q500GJD; one level down, Q420GJD.

Q460GJDZ15, Q460GJDZ25 and Q460GJDZ35: Through-Thickness Plate

A weld on the face of a thick plate shrinks and pulls the plate apart through its thickness. If the steel holds sulfide stringers, it tears in steps. Z15, Z25 and Z35 prove through-thickness ductility with a short-transverse tensile test.

The designation adds the Z level to the grade, for example Q460GJDZ25. Z tests apply to plate 15 mm and thicker and follow GB/T 5313-2023.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

The D melt already caps S at 0.010%, the Z15 limit, so Z25 and Z35 are the levels that change the steelmaking.

GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.

Most projects need Z only on flange and diaphragm plates over about 25–40 mm. Put the Z level on those items alone and keep the rest standard Q460GJD.

Equivalent Material Grades

ASTM A913 Gr.65 is the US high-strength seismic shape grade; it is a section standard, not plate. For plate, A572 Gr.65 is the strength comparison.

Designation Region Standard Notes
Q460GJD China GB/T 19879-2023 Grade on this page
EN 10025-4 S460M Europe EN 10025-3/-4 Strength match; no yield cap
EN 10025-3 S460N Europe EN 10025-3/-4 Alternative route
EN 10025-6 S460Q Europe EN 10025-6 QT; holds yield to 50 mm
GB/T 1591 Q460ND China GB/T 1591-2018 General structural
GB/T 16270 Q460D China GB/T 16270 QT plate
ASTM A572 Gr.65 USA ASTM A572 450 MPa; one step lower
JIS G3106 SM570 Japan JIS G3106 About 450–460 MPa; −5°C impact

On EN projects we usually quote Q460GJD against S460M or S460ML, because the TMCP route also gives the lowest CEV. See EN 10025-4 and EN 10025-6.

Weldability

GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q460GJD certificate:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Delivery condition CEV ≤ 50 mm CEV > 50 – 100 mm CEV > 100 – 150 mm Pcm ≤ 50 mm Pcm > 50 – 100 mm Pcm > 100 – 150 mm
CR, NR, N, NT 0.52 0.54 0.56 0.32 0.34 0.35
QT 0.45 0.48 0.50 0.28 0.30 0.31
TMCP, TMCP+T 0.42 0.45 By agreement 0.27 By agreement —

Q460GJ needs a written procedure. Published work on thick Q460GJC site welding reports preheat around 120°C, with interpass control and low-hydrogen consumables. Use that as context, not as your WPS.

The D letter helps: carbon is capped at 0.18% and P and S are lower, which reduces hot-cracking and HAZ embrittlement risk.

Typical consumables: E55- or E62-class low-hydrogen electrodes (GB/T 5118) or matching gas-shielded and SAW wires. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.

Heat Treatment and Delivery Condition

Q460GJD may be delivered CR, NR, N or NT, QT, or TMCP / TMCP+T. QT is also permitted. Each route has its own CEV and Pcm limits, so the route is part of the specification, not a mill detail.

TMCP gives the lowest CEV and the best weldability. N or NT gives the most uniform through-thickness properties on heavy plate. QT holds strength in the thickest sizes.

Agree the route before price. A mill quoting N where the drawing assumed TMCP CEV is not quoting the same plate. TMCP references: GB/T 1591 Q460MD; normalized: GB/T 1591 Q460ND.

Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.

Dimensions

Typical Q460GJD dimensions on our offers:

  • Thickness: 6 mm – 150 mm; most orders 8 mm – 100 mm
  • Width: 1500 mm – 3000 mm standard; wider by mill confirmation
  • Length: 3000 mm – 12000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³

Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.

Tolerances

GB/T 709-2019 governs Q460GJD thickness, width, length and flatness. Under Class B, the default, plate may be up to 0.30 mm thin and the plus side grows with thickness and width. Class C gives zero minus by agreement.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.

Supplementary Requirements

Q460GJD already fixes strength, yield ratio, CEV and −20°C impact. Anything more goes on the purchase order.

  • Edition: GB/T 19879-2023 or -2015. Never write only Q460.
  • Product analysis: ask for a second chemistry column checked to GB/T 222.
  • Through-thickness: add Z15, Z25 or Z35, e.g. Q460GJDZ25.
  • Delivery condition: name it (CR, NR, N, NT, QT, TMCP or TMCP+T) if the welding procedure depends on it.
  • Ultrasonic testing beyond Z plates: GB/T 2970 class, or EN 10160 / ASTM A578.
  • Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the D letter.
  • Tolerance: Class C for zero minus.
  • Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.

Q460GJD Price Factors and How to Order

There is no single Q460GJD price. Mills price GJ plate as base plus extras, and the order details set the extras.

Cost driver Effect on price
GJ grade over general Q460 plate Grade extra for cleaner steel, yield control and CEV
Quality letter D Extra for −20°C testing and the cleaner D melt
Delivery route QT and TMCP carry the largest route extras
Thickness Thin and very thick plate carry size extras; 10–60 mm is usually cheapest
Z15 / Z25 / Z35 Desulfurization, plate-by-plate Z test and UT; Z35 costs most
Width and length Over 3000 mm wide or 12 m long needs mill confirmation
Quantity per size Mill rolling minimums per size; small lots come from stock or combined rolling
Inspection and cutting 3.2 witness, profile cutting, blasting and priming are quoted per item

To get a firm quote in one round, send:

  • Grade and edition, e.g. Q460GJDZ25 to GB/T 19879-2023
  • Thickness × width × length and pieces or tonnes
  • Delivery route, UT standard and class
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q460GJE.

Applications

Sector Typical Q460GJD components
Super-tall towers Mega-columns, outrigger nodes, heavy splices
Stadium and terminal roofs Main truss chords and support nodes
Transfer structures Heavily loaded transfer and hanger plates
Steel-concrete composite Plate for encased or concrete-filled mega-columns

D grade covers severe winters, thick welded nodes and members erected in sub-zero weather.

It is the wrong plate for pressure equipment (pressure vessel steel plates), for bare exposed steel (weathering steel plates) or for ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q460GJD from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Xinyu, Valin Xiangtan, Shougang, Puyang and Hongchang when size requires.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
  • Tests: tensile, −20°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill

Buyers of Q460GJD are usually EPC contractors and fabricators working to Chinese drawings overseas. We ship to the United States, Europe, the Middle East, Southeast Asia, Africa and South America.

Lead time: stock sizes about 5–7 days; mill rolling about 30–45 days; Z35 or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.

Why Choose SHH STEEL

As a steel manufacturer and exporter and global steel mill sourcing partner, SHH STEEL buys Q460GJD straight from GJ-qualified mills, China origin. No relabelled general plate, no mixed heats.

Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio within the cap, CEV inside the thickness band for the delivery route, and −20°C impact at 47 J or more. If one fails, the plate does not ship as GJ.

We also tell buyers when they are over-specifying. If the design can live with 420 MPa, Q420GJD saves preheat and price. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q460GJD steel?
Q460GJD is high-performance building structure steel plate to GB/T 19879. It has 460 MPa minimum yield, a 460–590 MPa yield window from 16 to 100 mm, yield ratio ≤0.85, CEV limits by delivery route and Charpy impact of at least 47 J at −20°C. GJ stands for gao jian, high-performance building steel.
What is the difference between Q460GJD and S460M?
S460M (EN 10025) has a 460 MPa minimum yield that falls with thickness and no yield cap or yield-ratio limit. Q460GJD (GB/T 19879-2023) holds 460–590 MPa from 16 to 100 mm, caps the yield ratio at 0.85, sets CEV by delivery route and needs 47 J at −20°C. They are comparable for strength, not interchangeable.
When should I specify Q460GJD instead of Q460GJC?
Specify Q460GJD when the lowest service or erection temperature reaches about −20°C, when plate is thick and heavily restrained, or when Z25/Z35 is ordered. D is tested at −20°C (47 J) and its melt is cleaner: C ≤0.18%, P ≤0.020%, S ≤0.010%, against P 0.025% and S 0.015% for C grade.
Which delivery route is best for Q460GJ thick plate?
For weldability, TMCP: CEV ≤0.42% to 50 mm and 0.45% to 100 mm. For the heaviest plate, QT holds strength through the thickness with CEV ≤0.50% to 150 mm. CR/N plate carries the highest CEV, 0.52–0.56%.
What does Q460GJDZ35 mean?
Q460GJDZ35 is Q460GJD plate with Z35 through-thickness properties to GB/T 5313-2023: average reduction of area at least 35%, no single value below 25%, and heat sulfur 0.005% max. It applies to plate 15 mm and thicker, resists lamellar tearing, and each Z plate is ultrasonic tested.
What is the ASTM or EN equivalent of Q460GJD?
For strength, Q460GJD is compared with EN 10025 S460N/M or S460Q, ASTM A572 Gr.65 (450 MPa) and JIS SM570. None is an exact equivalent: they have no 590 MPa yield cap or 0.85 yield-ratio limit, which GB/T 19879-2023 requires for Q460GJD.

Conclusion

Q460GJD steel plate to GB/T 19879 is building structure plate with 460 MPa minimum yield, a capped yield window, a yield-ratio limit and 47 J impact at −20°C. It shares its chemistry with Q460GJB but proves toughness at its own letter. It is not general structural plate under GB/T 1591.

With SHH STEEL the Q460GJD certificate is complete: heat chemistry, CEV, yield, tensile, yield ratio and Charpy impact, to EN 10204 3.1 or 3.2. Add product analysis to GB/T 222, a Z15, Z25 or Z35 level, a GB/T 2970 UT class, Class C tolerance or profile cutting as the project needs.

We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.

Tell us the grade edition, sizes, tonnage and any Z, UT or inspection needs. We check the request against the standard first, then confirm mill, route, lead time and price. Contact SHH STEEL today for a mill-direct quotation on Q460GJD building steel plate.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X